Copper-doped graphene ink, preparation method and application thereof

By using copper-doped graphene ink in the plastic electroplating process, the pollution and high cost problems of hexavalent chromium and precious metal palladium in the prior art are solved, and plastic electroplating treatment with high adhesion and mirror effect is achieved.

CN116239915BActive Publication Date: 2024-11-08XIAMEN XIHE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211694985.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-08
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The use of hexavalent chromium and precious metal palladium in existing plastic electroplating processes leads to environmental pollution and high costs, and it is difficult to achieve the requirements of adhesion and mirror effects.

Method used

Copper-doped graphene ink, including graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and antioxidant micron copper, is coated on the substrate through electroplating pre-treatment technology to form conductive Layer to improve adhesion and mirror gloss.

Benefits of technology

It effectively avoids the use of hexavalent chromium and precious metal palladium, reduces costs, improves adhesion and mirror gloss effect, and is suitable for functional plastic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure BDA0004023044410000021
    Figure BDA0004023044410000021
Patent Text Reader

Abstract

The present invention provides a copper-doped graphene ink, comprising: 5 to 15 parts by weight of graphene; 0.5 to 5 parts by weight of conductive filler; 12 to 45 parts by weight of binder; 0.5 to 2 parts by weight of hydrophilic oxide; 25 to 48 parts by weight of high boiling point solvent; and 5 to 20 parts by weight of anti-oxidation micron copper. Compared with the prior art, the ink provided by the present invention can be conductive after curing, so that it can be electroplated. The anti-oxidation micron copper in the ink can not only improve the conductivity, but also serve as an active site for electroplating to improve the adhesion of the coating, thereby solving the pollution problem of hexavalent chromium in industry and further reducing the cost problem. It is suitable for various functional plastic products that need electroplating, and the adhesion can meet the requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electroplating technology, and in particular relates to a copper-doped graphene ink, a preparation method and application thereof. Background Art

[0002] Surface metal coating technology is a surface engineering technology for decorating, protecting and obtaining certain special properties on the substrate surface. It is also a metal deposition technology.

[0003] Surface metal plating technology can be divided into wet plating and dry plating. Among them, wet plating can be divided into chemical plating, electroplating and hot dip plating. Chemical plating is a self-catalytic plating method that does not require electricity. Based on the principle of redox reaction, a strong reducing agent is used in a solution containing metal ions to reduce metal ions to metals and deposit them on the surface of various materials to form a dense coating. The electroplating process is an electrochemical reduction process that occurs at the interface between metal and electrolyte. The prerequisite is to ensure sufficient contact between the electrolyte and the metal. The purpose of chemical plating is to generate a conductive metal film (usually copper or nickel plating) on ​​the surface of plastic products to create conditions for electroplating the metal layer of plastic products.

[0004] In order to obtain a good coating with good bonding and different surface textures, the current industry still uses the traditional roughening-activation-chemical plating conductive pre-treatment and then electroplating process. However, the hexavalent chromium used in the roughening process seriously pollutes the environment and has obvious irreversible damage to front-line workers who are directly in contact with it. Relevant countries and regions also have increasingly stringent restrictions on the use of hexavalent chromium. In addition, the use of precious metal palladium in the activation process and the need to meet relevant environmental standards have led to the continuous increase in the electroplating cost and wastewater treatment cost of electroplating plants. The plastic electroplating industry is in urgent need of a green and environmentally friendly production process.

[0005] At present, the main research directions for developing new environmentally friendly plastic electroplating processes are: (1) adjusting the etchant composition to avoid the use of hexavalent chromium, such as using manganese dioxide instead of chromic acid, increasing the amount of sulfuric acid to avoid the use of chromic acid, and hydrogen peroxide / nitric acid instead of chromic acid. Although these solutions avoid the use of hexavalent chromium, the roughening effect is poor, the yield is low, and the final adhesion is far from meeting the actual application requirements; (2) modifying the substrate surface, such as adding P-TES (6-azide-2,4-bis(3-triethoxy) The method comprises the following steps: grafting N-TES (6-azide-2,4-dithiol monosodium (3-triethoxysilyl)propylamino-1,3,5-triazine) molecules onto a plastic substrate by UV (ultraviolet light), grafting N-TES (6-azide-2,4-dithiol monosodium (3-triethoxysilyl)propylamino-1,3,5-triazine) molecules onto a plastic surface by self-assembly to form a molecular bond, chemically spraying Ag, and adsorbing the Ag film on the organic functional groups after the molecular bond, and then electroplating, or hydrolyzing and modifying the cyanide groups on the surface of ABS (acrylonitrile-butadiene-styrene copolymer) using a sodium hydroxide solution. The first method is to use a carboxyl group, which absorbs silver ions instead of palladium activation, and then electrolessly plate copper to complete the conductive pretreatment, or graft PAA (polyacrylic acid) to the plastic surface, and PAA absorbs copper ions, and then is reduced to complete the conductive pretreatment. This scheme can avoid the use of hexavalent chromium and precious metal palladium, but the steps are relatively complicated, the cost is also high, and the adhesion that the substrate surface can provide is also limited; (3) Conductive plastic, conductive materials are doped into the plastic substrate, and the materials are blended to form a conductive plastic substrate. This scheme can avoid the use of hexavalent chromium and precious metal palladium, but the addition of conductive materials will affect the mechanical properties of the plastic itself, and the conductivity needs to be improved, and good adhesion cannot be guaranteed; (4) Prepare a conductive slurry and coat it on the plastic substrate. This scheme avoids the use of hexavalent chromium and precious metal palladium, and has the advantages of simple process and suitability for large-scale industrial production. However, the difficulty of existing reports is still that the adhesion cannot meet the actual application requirements, and it is even more difficult to electroplate a good mirror gloss for decorative plastic electroplating workpieces that require a mirror effect. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a copper-doped graphene ink with strong adhesion and suitable for electroplating conductive treatment of decorative plastics that require a mirror effect, and a preparation method and application thereof.

[0007] The present invention provides a copper-doped graphene ink, comprising:

[0008]

[0009] Preferably, the conductive filler is selected from one or more of carbon black, silver nanoparticles and nickel nanoparticles;

[0010] The binder is selected from one or more of polyurethane, acrylic resin, phenolic resin and epoxy resin;

[0011] The boiling point of the high boiling point solvent is greater than 150°C.

[0012] Preferably, the hydrophilic oxide is selected from hydrophilic silicon dioxide.

[0013] Preferably, the high boiling point solvent is selected from one or more of dimethylformamide, N-methylpyrrolidone and dibasic acid ester.

[0014] Preferably, including:

[0015]

[0016] The present invention also provides a method for preparing the copper-doped graphene ink, comprising:

[0017] Graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and anti-oxidation micron copper are mixed to obtain copper-doped graphene ink.

[0018] The present invention also provides application of the copper-doped graphene ink in electroplating pre-treatment technology.

[0019] The present invention also provides an electroplating method, comprising:

[0020] The copper-doped graphene ink is coated on a substrate and then electroplated.

[0021] Preferably, the copper-doped graphene ink is coated to a thickness of 10 to 200 microns.

[0022] Preferably, the electroplating specifically comprises: sequentially performing cyanide-free pyrophosphate copper plating, bright copper plating and semi-bright nickel plating.

[0023] The present invention provides a copper-doped graphene ink, comprising: 5 to 15 parts by weight of graphene; 0.5 to 5 parts by weight of conductive filler; 12 to 45 parts by weight of binder; 0.5 to 2 parts by weight of hydrophilic oxide; 25 to 48 parts by weight of high boiling point solvent; and 5 to 20 parts by weight of anti-oxidation micron copper. Compared with the prior art, the ink provided by the present invention can be conductive after curing, so that it can be electroplated. The anti-oxidation micron copper in the ink can not only improve the conductivity, but also serve as an active site for electroplating to improve the adhesion of the coating, thereby solving the pollution problem of hexavalent chromium in industry and further reducing the cost problem. It is suitable for various functional plastic products that need electroplating, and the adhesion can meet the requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a laser microscope test image showing the shape measurement of the conductive ink cured layer prepared in Example 1 of the present invention and Comparative Example 1;

[0025] Figure 2 This is a mirror gloss effect diagram of the conductive plastic substrate prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] The invention provides a copper-doped graphene ink, comprising: 5-15 parts by weight of graphene; 0.5-5 parts by weight of conductive filler; 12-45 parts by weight of binder; 0.5-2 parts by weight of hydrophilic oxide; 25-48 parts by weight of high boiling point solvent; and 5-20 parts by weight of anti-oxidation micron copper.

[0028] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.

[0029] The content of graphene in the copper-doped graphene ink provided by the present invention is preferably 5 to 12 parts by weight, and more preferably 6 to 10 parts by weight.

[0030] The copper-doped graphene ink provided by the present invention includes a conductive filler, which can be filled between graphene sheets to improve conductivity; the content of the conductive filler in the copper-doped graphene ink is preferably 1 to 5 parts by weight, more preferably 1 to 4 parts by weight, and even more preferably 2 to 3 parts by weight; the type of the conductive filler can be any conductive filler well known to those skilled in the art, without any special restrictions, and in the present invention, preferably one or more of carbon black, silver nanoparticles and nickel nanoparticles.

[0031] The content of the binder in the copper-doped graphene ink provided by the present invention is preferably 15 to 45 parts by weight, more preferably 20 to 40 parts by weight, more preferably 30 to 40 parts by weight, and most preferably 35 to 40 parts by weight; the type of the binder can be a resin that can be used as a binder and is well known to those skilled in the art, and there is no special restriction. In the present invention, it is preferably one or more of polyurethane, acrylic resin, phenolic resin and epoxy resin, and more preferably polyurethane; in the present invention, the molecular weight of the polyurethane is preferably 2000 to 10000, more preferably 4000 to 8000, more preferably 6000 to 7000, and most preferably 6500; the tensile strength of the polyurethane is preferably 50 to 100 MPa, more preferably 60 to 90 MPa, and more preferably 70 to 80 MPa.

[0032] Adding hydrophilic oxides to the ink can improve the hydrophilicity of the ink, ensure that the film layer has good hydrophilicity, and enable the electroplating solution to infiltrate the inside of the film layer. In the subsequent electroplating, the metal ions in the electroplating solution are reduced to form an alloy with the anti-oxidation micron copper in the film layer, thereby ensuring good adhesion. The content of the hydrophilic oxide in the copper-doped graphene ink is preferably 0.8 to 1.5 parts by weight, and more preferably 1 part by weight; the hydrophilic oxide is preferably hydrophilic silica, and more preferably hydrophilic fumed silica; in the embodiments provided by the present invention, hydrophilic fumed silica A380 is specifically used as an example for explanation; hydrophilic silica can not only make the ink layer formed by the copper-doped graphene ink have a certain hydrophilicity, but also effectively reduce the resistivity change caused by resin swelling, and can also improve the mechanical strength of the ink layer itself.

[0033] The copper-doped graphene ink provided by the present invention adopts a high boiling point solvent, which can dissolve the resin well and evaporate slowly. After drying, a flat ink layer can be easily obtained, and the relatively flat surface is convenient for forming a flat, mirror-like glossy coating after electroplating. Among them, the content of the high boiling point solvent in the copper-doped graphene ink is preferably 28 to 45 parts by weight, more preferably 30 to 40 parts by weight, and more preferably 31 to 38 parts by weight; in the present invention, the boiling point of the high boiling point solvent is preferably greater than 150°C; the high boiling point solvent is preferably one or more of dimethylformamide (DMF), N-methylpyrrolidone (NMP) and dibasic acid ester (DBE).

[0034] The copper-doped graphene ink provided by the present invention contains anti-oxidation micron copper, which is used to provide electroplating active sites, and the use of micron copper with anti-oxidation function can maintain the stability of the ink for a long time. The content of the anti-oxidation micron copper in the copper-doped graphene ink is preferably 5 to 15 parts by weight, more preferably 5 to 10 parts by weight, and more preferably 5 to 8 parts by weight; the anti-oxidation micron copper can be micron copper particles with anti-oxidation properties well known to those skilled in the art, and there is no special restriction. In the present invention, it is preferably anti-oxidation micron copper prepared according to the method in the Chinese patent with publication number CN113707362A.

[0035] The ink provided by the present invention can be made conductive after being cured, so that it can be electroplated. The anti-oxidation micron copper in the ink can not only improve the conductivity, but also serve as an electroplating active site to improve the adhesion of the coating, thereby solving the pollution problem of hexavalent chromium in industry and further reducing the cost problem. The ink is suitable for various functional plastic products that need to be electroplated, and the adhesion can meet the requirements. For decorative plastic electroplating workpieces that need to have a mirror effect, good mirror gloss can also be electroplated.

[0036] The present invention also provides a method for preparing the copper-doped graphene ink, comprising: mixing graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and anti-oxidation micron copper to obtain the copper-doped graphene ink.

[0037] The contents and types of the graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and antioxidant micron copper are the same as described above and will not be repeated here.

[0038] Graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and antioxidant micron copper are mixed; the mixing method is a method well known to those skilled in the art and is not particularly limited. In the present invention, ball milling or sand milling is preferred; the mixing time is preferably 0.5 to 3 hours; the mixing speed is preferably 200 to 500 rpm, more preferably 300 to 400 rpm, and more preferably 350 rpm; the ball-to-material ratio of the ball milling or sand milling is preferably 1 to 1.5, and more preferably 1.1; the grinding balls used for the ball milling or sand milling preferably include grinding balls of different diameters, wherein the volume ratio of large balls to small balls is preferably (3 to 6):1, more preferably (4 to 5):1, and more preferably 5:1; the diameter of the large balls is preferably 8 to 15 mm, and more preferably 10 mm; the diameter of the small balls is preferably 3 to 6 mm, and more preferably 5 mm.

[0039] The present invention also provides an application of the copper-doped graphene ink in electroplating pretreatment technology. The copper-doped graphene ink provided by the present invention can be directly electroplated after being cured into a film, thereby solving the pollution problem of hexavalent chromium in industry and further reducing the cost problem, and is suitable for decorative products that require mirror gloss.

[0040] The present invention also provides an electroplating method, comprising: coating the copper-doped graphene ink on a substrate, and then performing electroplating.

[0041] The copper-doped graphene ink is coated on a substrate; the coating method is a method well known to those skilled in the art, such as scraping, spraying, dipping, etc., without any special restrictions; the coating thickness is preferably 10 to 200 microns (after drying), more preferably 20 to 150 microns, more preferably 40 to 100 microns, and most preferably 60 to 70 microns; the substrate is a substrate well known to those skilled in the art, without any special restrictions, and in the present invention, a non-conductive ABS plastic substrate is preferably used.

[0042] After coating, the film is cured; the film curing method is a method well known to those skilled in the art, and there is no special limitation on natural drying, blow drying, baking and the like. In the present invention, baking is preferred; the drying temperature is preferably 40°C to 80°C, more preferably 50°C to 60°C; the drying time is preferably 1 to 3 hours.

[0043] Then electroplating is carried out; the electroplating process is an electroplating process well known to those skilled in the art and is not particularly limited. In the present invention, it is preferred to select a plating solution with less impact on the environment, specifically, firstly carry out cyanide-free pyrophosphate copper plating; the electroplating solution used for the cyanide-free pyrophosphate copper plating preferably includes: 17-18 parts by weight of pyrophosphate, 5.5-6 parts by weight of copper salt, 5-6 parts by weight of buffer salt, 0.6-1 part by weight of ammonia water, 0.1-0.3 parts by weight of polyethylene glycol and 70-71 parts by weight of water; the pyrophosphate is preferably potassium pyrophosphate; the copper salt is preferably copper sulfate; the buffer salt is preferably dipotassium hydrogen phosphate; the polyethylene glycol is preferably polyethylene glycol-600; the current density of the cyanide-free pyrophosphate copper plating is preferably 0.5-1ASD; the time of the cyanide-free pyrophosphate copper plating is preferably 10-20min; using pyrophosphate copper plating as a base coating can improve the bonding strength between the coating and the substrate, and further adopting a cyanide-free process is green and environmentally friendly.

[0044] After the cyanide-free pyrophosphate copper plating, it is preferred to further electroplate bright copper to obtain a coating with high corrosion resistance; the plating solution used for the electroplating of bright copper can be a plating solution well known to those skilled in the art, and there is no special limitation. The acid copper plating solution used for the electroplating of bright copper in the present invention preferably includes 180-200 g / L of copper sulfate, 62-68 g / L of sulfuric acid, and 80-100 ppm of chloride ions; the current density of the electroplating of bright copper is preferably 2-6 ASD; the time of the electroplating of bright copper is preferably 10-30 min.

[0045] After electroplating bright copper, it is preferred to also electroplating semi-bright nickel; the plating solution used for the electroplating semi-bright nickel preferably includes 220-240 g / L of nickel sulfate, 60-70 g / L of nickel chloride, and 40-50 g / L of boric acid; the current density of the electroplating semi-bright nickel is preferably 1-2 ASD; the time for the electroplating semi-bright nickel is preferably 5-10 min.

[0046] In the present invention, according to product requirements, electroplating may be further performed subsequently, such as full-bright nickel, microporous nickel, bright chromium, etc.

[0047] After electroplating, drying is preferably performed; residual moisture in the micropores of the ink layer can be removed by drying to obtain a coating with good adhesion; the drying is preferably vacuum drying; the drying temperature is preferably 40°C to 100°C, more preferably 60°C to 80°C; the drying time is preferably 6 to 24 hours.

[0048] Compared with the traditional electroplating process, the present invention uses a copper-doped graphene ink coated on a non-conductive plastic substrate to achieve conductive treatment instead of the traditional degreasing-roughening-activation-chemical plating conductive pretreatment method, which can avoid the use of hexavalent chromium in the roughening process and the use of precious metal palladium in the activation process. In addition, it also simplifies the complex process of degreasing, neutralization, degumming, chemical plating, etc., which is not only environmentally friendly, but also greatly reduces the cost.

[0049] In order to further illustrate the present invention, a copper-doped graphene ink, a preparation method thereof and applications provided by the present invention are described in detail below in conjunction with embodiments.

[0050] The reagents used in the following examples are all commercially available. The antioxidant micron copper powder used in the examples is C-1 prepared in the Chinese patent with publication number CN113707362A; the hydrophilic silica used in the examples and comparative examples is A380 hydrophilic fumed silica purchased by Degussa; the molecular weight of the polyurethane is 6500, the tensile strength is 70 MPa, and the 100% modulus is 4.5; the graphene is 8 μm high-purity expanded graphite purchased by Qingdao Yanhai Carbon Materials Co., Ltd.; the carbon black is Cabot BLACK PEARLS 2000 superconductive carbon black purchased by Cabot, USA; the nickel powder is 10 μm flaky conductive nickel powder purchased by Shanghai Naio Nano Technology Co., Ltd.; ABS is purchased by Xiamen Jianlin Healthy Home Co., Ltd.; the ordinary micron copper powder is 1000 mesh high-purity copper powder purchased by Nangong Ruili Alloy Welding Materials Co., Ltd.

[0051] Example 1

[0052] Preparation of copper-doped graphene ink: 10 parts of graphene, 8 parts of antioxidant micron copper powder, 3 parts of carbon black, 1 part of hydrophilic silica, 40 parts of polyurethane, and 38 parts of DMF. After mixing, use a planetary ball mill at 350 rpm for 3 hours (using a large ball with a diameter of 10 mm and a small ball with a diameter of 5 mm for mixed ball milling (large ball: small ball = 5:1, ball-to-material ratio (by volume) = 1.1) to obtain copper-doped graphene ink.

[0053] Preparation of conductive ink solidified layer: The copper-doped graphene ink was transferred to a non-conductive plastic substrate (ABS) by spraying, and the slurry was cured into a film by drying at 60°C for 2 h.

[0054] Preparation of conductive plastic substrate: Use cyanide-free alkaline pyrophosphate copper plating solution at 1A / dm 2 Electroplating for 10 minutes, bright acid copper plating solution at 6A / dm 2 Electroplating for 30 minutes, semi-bright nickel plating solution at 2A / dm 2 The electroplating was performed for 5 minutes. The components of the electroplating solution used are shown in Tables 1 to 3.

[0055] Table 1 Composition of copper pyrophosphate plating solution

[0056]

[0057] Table 2 Bright Acid Copper Plating Solution Composition

[0058]

[0059] Table 3 Semi-bright nickel plating solution composition

[0060]

[0061] Post-processing parameters: drying at 60℃ under vacuum conditions for 24h.

[0062] Comparative Example 1

[0063] Preparation of conductive ink: 10 parts of graphene, 8 parts of ordinary micron copper powder, 3 parts of carbon black, 1 part of hydrophilic silica, 40 parts of polyurethane, and 38 parts of DMF.

[0064] The preparation of the conductive ink cured layer and the conductive plastic substrate are the same as those in Example 1.

[0065] Comparative Example 2

[0066] Preparation of conductive ink: 10 parts of graphene, 8 parts of nickel powder, 3 parts of carbon black, 1 part of hydrophilic silica, 40 parts of polyurethane, and 38 parts of DMF.

[0067] The preparation of the conductive ink cured layer and the conductive plastic substrate are the same as those in Example 1.

[0068] Comparative Example 3

[0069] Preparation of conductive ink: 10 parts of graphene, 8 parts of antioxidant copper powder, 3 parts of carbon black, 1 part of hydrophilic silica, 40 parts of polyurethane, and 38 parts of NMP.

[0070] The preparation of the conductive ink cured layer and the conductive plastic substrate are the same as those in Example 1.

[0071] Comparative Example 4

[0072] The conductive pretreatment is a conventional etching-activation-chemical plating process, and the electroplating conditions are the same as those in Example 1, specifically as follows: (1) alkaline degreasing: NaOH: 50 g / L, Na3PO4: 30 g / L, Na2CO3: 15 g / L, temperature: 40-45°C, time: 5 min; (2) swelling: acetone: water = 1:2 (volume ratio), temperature: room temperature, time: 15 min; (3) coarsening: CrO3: 400 g / L, H2SO4: 350 g / L, temperature: 50-75°C, time: 60 min; (4) alkaline washing: 10% (mass fraction) NaOH solution, temperature: room temperature, time: 5 min; (5) Sensitization: SnCl2·2H2O: 15g / L, HCl: 45ml / L, temperature: room temperature, time: 5min; (6) Activation: PbCl2: 0.5g / L; HCl: 10ml / L, temperature: room temperature, time: 1~3min; (7) Chemical copper plating: CuSO4·5H2O: 15g / L, p-toluenesulfonic acid ammonium: 20~22g / L, potassium sodium tartrate: 60g / L, formaldehyde: 0.06~0.15g / L, nickel chloride: 2g / L, NaOH: 10~15g / L, formaldehyde: 8~18g / L, temperature: 25℃, time: 20min.

[0073] Performance Testing

[0074] 1. Conductive ink performance test

[0075] The conductive inks prepared in Example 1 and Comparative Examples 1 to 3 were respectively subjected to resistivity tests and sheet resistance tests, and the results are shown in Table 4. As can be seen from Table 4, compared with Comparative Examples 1 to 3, the sheet resistance and resistivity of the conductive ink layer after electroplating prepared in Example 1 are lower, and the conductivity is better.

[0076] Table 4 Test results of resistivity / sheet resistance of conductive ink prepared in Example 1 and Comparative Examples 1 to 3

[0077]

[0078] 2. Conductive ink curing layer performance test

[0079] The surface roughness of the cured conductive ink layer prepared in Example 1 and Comparative Example 4 was measured by laser microscope. The surface morphology is shown in Figure 1 The surface roughness Sa of the conductive ink layer prepared in Example 1 after curing was measured to be 4.9063 μm, and the surface roughness Sa of the conductive ink layer prepared in Comparative Example 4 after curing was measured to be 5.4680 μm. Figure 1 It can be seen that the conductive ink layer after curing prepared in Example 1 is relatively flat, and its surface morphology is similar to that of the ink layer prepared in Comparative Example 4 using the traditional etching-activation-chemical plating process.

[0080] The conductive ink cured layers prepared in Example 1 and Comparative Examples 1 to 3 were subjected to a square resistance test and a grid test (ASTM D3359 standard test method), respectively. The results are shown in Table 5.

[0081] Table 5 Performance test results of the conductive ink cured layer prepared in Example 1 and Comparative Examples 1 to 3

[0082]

[0083] As can be seen from Table 5, the conductive ink cured layer prepared in Example 1 and Comparative Examples 1 to 3 have comparable results in the 100-grid test, and the conductive ink cured layer prepared in Example 1 can meet the requirements of commercial applications. Compared with Comparative Examples 1 to 3, the conductive ink cured layer prepared in Example 1 has lower square resistance and better conductivity.

[0084] 3. Conductive plastic substrate performance test

[0085] The conductive plastic substrates prepared in Example 1 and Comparative Examples 1 to 3 were subjected to a hundred-grid test (ASTM D3359 standard test method and a 90° tensile test (ASTM B533-85 (2013) standard test method), respectively. The results are shown in Table 6.

[0086] Table 6 Performance test results of conductive plastic substrates prepared in Example 1 and Comparative Examples 1 to 3

[0087]

[0088] As can be seen from Table 6, the conductive plastic substrates prepared in Example 1 and Comparative Examples 1 to 3 have comparable results in the 100° test, and the conductive plastic substrate prepared in Example 1 is significantly better than Comparative Examples 1 to 3 in the 90° tensile test, indicating that the antioxidant copper particles added to the conductive ink can act as active sites for electroplating, providing nucleation sites for subsequent electroplated copper, and the newly deposited copper and the copper in the original ink form metal bonds, which significantly improves the adhesion of the film layer and can be used in more stringent use environments. At the same time, the conductive plastic substrate prepared in Example 1 has a higher brightness and can be used for decorative products that require a mirror gloss. The mirror effect can be seen in Figure 2 .

Claims

1. A copper-doped graphene ink, characterized in that: It is composed of the following components: 5 to 15 parts by weight of graphene; 0.5 to 5 parts by weight of conductive filler; 12 to 45 parts by weight of binder; 0.5 to 2 parts by weight of hydrophilic oxide; 25 to 48 parts by weight of a high boiling point solvent; 5-20 parts by weight of anti-oxidation micron copper; The hydrophilic oxide is selected from hydrophilic silicon dioxide; The boiling point of the high boiling point solvent is greater than 150°C; The copper-doped graphene ink is applied in electroplating pre-treatment technology; The conductive filler is selected from one or more of carbon black, silver nanoparticles and nickel nanoparticles; The binder is selected from one or more of polyurethane, acrylic resin, phenolic resin and epoxy resin; The high boiling point solvent is selected from one or more of dimethylformamide, N-methylpyrrolidone and dibasic acid ester.

2. The copper-doped graphene ink according to claim 1, characterized in that: include: 8 to 12 parts by weight of graphene; 0.5 to 5 parts by weight of conductive filler; 35-40 parts by weight of binder; 0.5 to 2 parts by weight of hydrophilic oxide; 38 to 46 parts by weight of a high boiling point solvent; 5 to 8 parts by weight of anti-oxidation micron copper.

3. A method for preparing the copper-doped graphene ink according to claim 1, characterized in that: include: Graphene, conductive filler, binder, hydrophilic oxide, high boiling point solvent and anti-oxidation micron copper are mixed to obtain copper-doped graphene ink.

4. Application of the copper-doped graphene ink according to claim 1 or 2 in electroplating pretreatment technology.

5. An electroplating method, characterized in that: include: The copper-doped graphene ink according to claim 1 or 2 is coated on a substrate and then electroplated.

6. The electroplating method according to claim 5, characterized in that: The copper-doped graphene ink is coated to a thickness of 10 to 200 microns.

7. The electroplating method according to claim 5, characterized in that: The electroplating specifically comprises: sequentially performing cyanide-free pyrophosphate copper plating, bright copper plating and semi-bright nickel plating.