Friction structural part for matching with polymer, preparation method and application thereof

By using Cr-doped composite coating in mechanical seals, the adhesion chemical reaction problem of amorphous carbon coating and polymer friction pairs is solved, and the friction running period is shortened and the friction coefficient is reduced, which has improved the application potential , and simplifies the production process.

CN116240492BActive Publication Date: 2024-11-26NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310241367.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-11-26
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

In mechanical seals, amorphous carbon coatings are prone to adhere chemical reactions when they rub against the polymer with the pair, resulting in an extended friction running period and an increased friction coefficient, limiting its application.

Method used

Using a composite coating with doped Cr elements, the Cr/CrN transition layer and Cr doped amorphous carbon layer are formed on the surface of the substrate, combined with high-power pulse magnetron sputtering and DC magnetron sputtering technology, at low matrix temperature Deposit a dense coating to inhibit the adhesion chemical reaction between free radicals on the surface of the polymer and amorphous carbon, forming a lubricating interface between metal and amorphous carbon.

Benefits of technology

It effectively shortens the friction running period, reduces the friction coefficient, maintains the excellent lubricity of the carbon-based coating, improves the application potential of the pairing, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116240492B_ABST
    Figure CN116240492B_ABST
Patent Text Reader

Abstract

The present invention discloses a friction structure for use with a polymer, a preparation method and an application thereof. The friction structure comprises a substrate and a composite coating disposed on the friction surface of the substrate, wherein the composite coating comprises a transition layer and an amorphous carbon layer stacked in sequence in a direction away from the substrate, wherein the amorphous carbon layer is doped with a Cr element. The present invention regulates the friction interface between the coating and the polymer by doping the metal element Cr, maintains the excellent lubricity of the carbon-based coating, does not affect the formation process of the amorphous carbon graphitized friction film, and can inhibit the adhesion chemical reaction, form an excellent metal and amorphous carbon lubrication interface, shorten the friction running-in period of the pair, reduce the friction coefficient, and increase the application potential of the pair; the preparation method provided combines high-power pulsed magnetron sputtering and DC magnetron sputtering technology, and can deposit a void-free, high-density composite coating at a low substrate temperature, with a safe operating environment and a simple and easy-to-control process, which is conducive to industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of surface protection technology, and in particular to a friction structural part for use with a polymer, a preparation method and application thereof, and specifically to a low-wear control structure and method for shortening the friction running-in period between a carbon-based coating and a polymer pair. Background Art

[0002] Mechanical seals, also known as face seals, are widely used in equipment such as pumps, reactors, compressors, and hydraulic transmissions. They are critical components of these machines and significantly impact their proper operation and safe production. Friction and wear of sealing materials are the primary cause of mechanical seal failure, leakage, and other accidents.

[0003] Soft sealing polymer materials commonly used in mechanical seals, such as polyetheretherketone (PEEK), polytetrafluoroethylene (PTFE), polyimide (PI) and polyphenylene sulfide (PPS), are often used as common solid lubricants in stainless steel-stainless steel friction systems to obtain a low friction coefficient due to their good anti-friction lubrication and sealing properties.

[0004] Researchers generally believe that one of the important functions of polymers in improving lubrication performance is to form a transfer film on the steel surface. 2 and sp 3 A metastable material formed by hybridization combines high hardness, wear resistance, and chemical inertness. Typically, during friction, the amorphous carbon coating transfers to the opposing metal surface, forming a graphitized tribofilm that provides friction-reducing and lubricating properties. Therefore, modifying metal components and polymer mating components with amorphous carbon coatings can achieve friction-reducing and lubrication in a variety of operating conditions, particularly those with stringent sealing requirements.

[0005] However, studies have confirmed that when these two materials with solid self-lubricating properties are rubbed together, serious adhesive chemical reactions will occur. For example, after PEEK friction, surface ether and diphenyl ether bonds are broken, forming ROC·, RO·, and RC· free radicals, which rebond with the C on the amorphous carbon surface. The above adhesive chemical reactions significantly affect the tribological properties of the friction pair.

[0006] Typically, for example, under dry friction conditions in the absence of liquid lubrication, the friction running-in period caused by adhesive chemical reactions may be as long as 5 hours, and the friction coefficient may reach as high as 0.55, which greatly limits the practical application of amorphous carbon coatings and polymer pairs. Summary of the Invention

[0007] In view of the deficiencies in the prior art, the present invention aims to provide a friction structural component for pairing with a polymer, a preparation method thereof and applications.

[0008] To achieve the aforementioned object of the invention, the technical solutions adopted by the present invention include:

[0009] In a first aspect, the present invention provides a friction structural part for pairing with a polymer, comprising a substrate and a composite coating arranged on the friction surface of the substrate, wherein the composite coating comprises a transition layer and an amorphous carbon layer stacked in sequence in a direction away from the substrate, and the amorphous carbon layer is doped with a Cr element.

[0010] In a second aspect, the present invention further provides a method for preparing the above-mentioned friction structural component, which comprises:

[0011] providing a substrate;

[0012] forming a transition layer on the friction surface of the substrate;

[0013] An amorphous carbon layer is formed on the surface of the transition layer, and the amorphous carbon layer is doped with Cr element.

[0014] In a third aspect, the present invention further provides a friction pair, comprising the above-mentioned friction structure and a friction body frictionally matched with the friction structure;

[0015] The material of the friction surface of the friction body includes polymer.

[0016] In a fourth aspect, the present invention further provides application of the above-mentioned friction pair in mechanical seals.

[0017] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention include at least:

[0018] The present invention regulates the friction interface between the coating and the polymer by doping the metal element Cr, which can maintain the excellent lubricity of the carbon-based coating without affecting the formation process of the amorphous carbon graphitized friction film. At the same time, it can inhibit the adhesion chemical reaction between the free radicals formed after friction on the polymer surface and the C on the amorphous carbon surface, forming an excellent metal-amorphous carbon lubrication interface, shortening the friction running-in period of the pairing, reducing the friction coefficient, and increasing the potential for the pairing to be applied in other fields.

[0019] The preparation method provided by the present invention combines high-power pulsed magnetron sputtering and DC magnetron sputtering technology to deposit void-free, high-density composite coatings at low substrate temperatures. The operating environment is safe and the process is simple and easy to control, which is conducive to industrial production applications.

[0020] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of this application and implement them according to the contents of the specification, the following is an explanation of the preferred embodiments of the present invention with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1This is the full XPS spectrum of the composite coating provided by some typical embodiments of the present invention;

[0022] Figure 2 The friction coefficient test graphs of the composite coatings provided by some typical implementation cases and comparative cases of the present invention are shown;

[0023] Figure 3 1. The friction coefficient test graphs of the composite coatings provided in other typical implementation cases and comparative cases of the present invention;

[0024] Figure 4a This is a surface SEM image of a composite coating provided in a typical comparative example of the present invention;

[0025] Figure 4b This is a surface SEM image of a composite coating provided by a typical embodiment of the present invention;

[0026] Figure 5 These are test diagrams of the bonding strength of composite coatings provided by some typical implementation cases and comparative cases of the present invention. DETAILED DESCRIPTION

[0027] In the prior art, amorphous carbon coating is made of carbon sp 2 With sp 3 A class of materials composed of hybrid bonds exhibits high hardness and elastic modulus, with a coefficient of friction as low as 0.03, making them a preferred material for precision mating protective coatings. However, empirically, the formation of a graphite transfer layer from the amorphous carbon coating to the metal counterpart is crucial for reducing the COF during sliding. However, previous studies have shown that friction between these two materials exhibiting solid self-lubricating properties can produce severe adhesive chemical reactions, significantly limiting the practical application of amorphous carbon coatings and polymer mating.

[0028] In view of the deficiencies in the prior art, the inventors of this case discovered through long-term research and extensive practice that doping with an appropriate amount of Cr content can form a metal transfer film on the polymer surface, transforming the friction interface between amorphous carbon and polymer into a friction interface between metal and amorphous carbon. It can also significantly inhibit adhesion chemical reactions, shorten the friction running-in period of the mating pair, and reduce the friction coefficient, thereby proposing the technical solution of the present invention.

[0029] The technical solution, its implementation process and principles are further explained below.

[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the scope of protection of the present invention is not limited to the specific embodiments disclosed below.

[0031] One aspect of an embodiment of the present invention provides a friction structural component for pairing with a polymer, comprising a substrate and a composite coating arranged on the friction surface of the substrate, wherein the composite coating includes a transition layer and an amorphous carbon layer stacked in sequence in a direction away from the substrate, and the amorphous carbon layer is doped with a Cr element.

[0032] In the above technical solution, the present invention relates to a low-wear control method for shortening the friction running-in period of a carbon-based coating and a polymer pair, and improves the lubrication behavior of the friction interface between the carbon-based coating and polyetheretherketone through a metal doping design. The metal doping design is a Cr-doped hydrogen-free carbon-based composite coating. In a very specific implementation case, the composite coating includes a Cr / CrN transition layer and a Cr-doped hydrogen-free amorphous carbon layer sequentially formed on the surface of a stainless steel substrate.

[0033] Furthermore, it is preferred to use a multi-target magnetron sputtering technique to prepare a metal-doped carbon-based composite coating on the surface of stainless steel, as specifically exemplified below.

[0034] The substrate can be a metal substrate, preferably a stainless steel substrate, more preferably, 316, 304, 17-4PH stainless steel, the best choice is 17-4PH stainless steel, and is not limited thereto. The main technical means of the technical solution provided by the present invention is that the Cr doping component and the high sp 2 The combination of the amorphous carbon layer with high carbon content brings about excellent running-in performance with the surface of the polymer material. The material selection of the substrate can be any substrate material that meets certain strength standards, such as ceramic materials or other metal materials, etc.

[0035] Depending on the material, the material selection for the transition layer may vary. Those skilled in the art can appropriately select a suitable transition layer based on common existing techniques to ensure good bonding between the substrate and the amorphous carbon layer. Therefore, the material selection and structure of the specific substrate and transition layer disclosed in the present invention are not limited to the specific examples below.

[0036] In some embodiments, the amorphous carbon layer is formed of a hydrogen-free amorphous carbon material formed by a mixture of a diamond phase and a graphite phase.

[0037] In some embodiments, the molar ratio of the diamond phase to the graphite phase in the amorphous carbon layer is 1:2 to 1:5.

[0038] In some embodiments, the atomic percentage of Cr in the amorphous carbon layer is preferably 2.15-15.52%, particularly preferably 2.15-4%. In the present invention, the Cr content greatly affects the hardness, modulus and internal stress of the Cr-doped amorphous carbon composite coating. If the Cr doping content in the amorphous carbon coating is too high, the hardness of the coating is too low, the resistance to plastic deformation is weak, and the anti-friction performance is reduced. An appropriate Cr content can inhibit the adhesion chemical reaction between the coating and the polymer friction interface and maintain a suitable mechanical property, thereby maintaining the wear resistance of the amorphous carbon coating while reducing the friction coefficient.

[0039] In some embodiments, the composite coating may have a thickness of 300-500 nm.

[0040] In some embodiments, the thickness of the transition layer may be 150-240 nm.

[0041] In some embodiments, the transition layer includes a Cr layer and a CrN layer stacked in sequence in a direction away from the substrate.

[0042] In some embodiments, the thickness of the Cr layer may be 80-120 nm, and the thickness of the CrN layer may be 80-120 nm.

[0043] In some embodiments, the amorphous carbon layer may have a thickness of 150-300 nm.

[0044] A second aspect of an embodiment of the present invention further provides a method for preparing a friction structural component in any of the above embodiments, comprising the following steps:

[0045] providing a substrate;

[0046] forming a transition layer on the friction surface of the substrate;

[0047] An amorphous carbon layer is formed on the surface of the transition layer, and the amorphous carbon layer is doped with Cr element.

[0048] In some embodiments, the preparation method specifically comprises:

[0049] Magnetron sputtering is used to sequentially deposit a Cr layer and a CrN layer on the substrate surface. In the present invention, since the hardness of the metal and amorphous carbon coatings differ significantly, and the hardness of CrN is between Cr and amorphous carbon, a three-layer structure with the CrN layer as the middle layer can effectively alleviate the interface mismatch problem and improve the coating adhesion.

[0050] The amorphous carbon layer is formed by co-deposition on the surface of the CrN layer by adopting direct current magnetron sputtering of a C target and pulsed magnetron sputtering of a Cr target.

[0051] In some embodiments, the sputtering method of the Cr layer and the CrN layer can be selected from DC magnetron sputtering.

[0052] In some embodiments, the substrate may be cleaned and etched before magnetron sputtering. The specific cleaning agent etching treatment is mainly to improve the bonding strength between the substrate and the composite coating to achieve the corresponding function, and is not limited to the cleaning / etching methods specifically exemplified in the following embodiments.

[0053] In some embodiments, the CrN layer can be deposited by introducing a nitrogen source on the basis of magnetron sputtering the Cr layer.

[0054] In some embodiments, the nitrogen source may include nitrogen gas.

[0055] In some embodiments, the Ar flow rate during deposition of the Cr layer and the CrN layer can be 45-65 sccm, the pulsed negative bias voltage can be 80-120 V, the chamber pressure can be 2.0-2.5 mTorr, the chamber temperature can be 130-170° C., and the deposition time can be 5-10 min.

[0056] In some embodiments, the N2 flow rate when depositing the CrN layer can be 15-25 sccm.

[0057] In some embodiments, the Ar flow rate when depositing the amorphous carbon layer can be 45-65 sccm, the pulse negative bias voltage can be 180-220 V, the DC current can be 2.5-3.5 A, the power of pulsed magnetron sputtering can be 100-400 W, and the deposition time can be 30-50 min.

[0058] As some typical application examples of the above technical solution, the following steps can be used to implement the above preparation method:

[0059] 1) Ultrasonic cleaning of the stainless steel substrate surface.

[0060] And, 2) using multi-target magnetron sputtering technology, the stainless steel substrate obtained after cleaning is placed in a reaction chamber and evacuated; Ar is introduced to etch the substrate, and then a Cr / CrN transition layer is prepared using a DC power supply. The process parameters include: Ar flow rate of 55 sccm, N2 flow rate of 20 sccm, pulse negative bias voltage of 100 V, chamber pressure of 2.0-2.5 mTorr, chamber temperature of 150°C, and deposition time of 8 min; finally, a DC power supply (DC) combined with high-power pulsed magnetron sputtering technology (HiPIMS) is used to deposit a Cr-doped amorphous carbon layer. The process parameters include: Ar flow rate of 55 sccm, pulse negative bias voltage of 200 V, DC current of 3.0 A, HiPIMS power of 100-300 W, and deposition time of 30-50 min.

[0061] The target materials used in the multi-target magnetron sputtering preferably include a Cr target and a C target with a purity of 99.99%.

[0062] Therefore, the technical solution exemplified in the present invention uses multi-target magnetron sputtering technology to form a Cr-doped amorphous carbon composite coating on the surface of a stainless steel substrate; DC magnetron sputtering combined with high-power pulsed magnetron sputtering technology is used to optimize the deposition process parameters, which can accurately control the Cr doping content, thereby inhibiting the adhesive chemical reaction at the interface between the coating and the polymer, shortening the friction running-in period, and reducing the friction coefficient, making it have great potential in the application of dry friction solid lubrication.

[0063] On this basis, as an application, the third aspect of an embodiment of the present invention further provides a friction pair, which includes the friction structure in any of the above embodiments and a friction body that frictionally cooperates with the friction structure; the material of the friction body on the friction surface includes a polymer.

[0064] In some embodiments, the polymer may include, for example, any one of PEEK, PTFE, PI, and PPS, or a combination of two or more thereof, but is not limited thereto.

[0065] In some embodiments, the friction pair is a dry friction pair.

[0066] In some embodiments, the running-in period of the friction pair is less than 30 minutes.

[0067] In some embodiments, after the running-in, the friction coefficient of the friction pair is below 0.2.

[0068] In a further application, as a fourth aspect of an embodiment of the present invention, there is also provided an application of the friction pair in any of the above embodiments in a mechanical seal. The coating structure provided by the present invention is very suitable for the field of mechanical seals with dynamic friction.

[0069] The inventors of the present invention noted that the prior art also provides some technical solutions for preparing chromium-doped amorphous carbon coatings using cathode arc equipment. However, the difference is that in the above-mentioned embodiment, the present invention uses a multi-target magnetron sputtering device to prepare the Cr-doped carbon-based coating. The positive ions generated by gas discharge bombard the target as the cathode under the action of the electric field, causing atoms (or molecules) in the target material to escape and deposit on the substrate surface to form the desired coating. The prior art uses a magnetically filtered vacuum cathode arc device, which uses arc discharge in a vacuum environment to evaporate the plating particles as the source of ion plating. The preparation methods and principles of the two are completely different.

[0070] Specifically, the Cr-doped carbon-based coating in the embodiment of the present invention is a high sp 2 The amorphous carbon coating with high content has high environmental adaptability and good lubrication performance. However, in the comparative document, due to the difference in preparation principle, the deionization rate is very high, and the carbon-based coating prepared is sp 3 The content is extremely high, and the desired technical effect can only be achieved by graphitizing the coating through heating or metal catalysis.

[0071] In terms of purpose, the present invention is mainly aimed at the system of carbon-based coating and polymer pairing. The purpose of Cr doping modification is to improve the lubrication performance of the polymer-carbon-based coating pairing system, and its main purpose is to reduce polymer wear; while the comparative document is mainly aimed at the surface protection of the metal material itself, so the specific effects of chromium doping in the two are not the same.

[0072] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0073] Example 1

[0074] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0075] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum with a degree of less than 4*10- 5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0076] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and the Cr layer was deposited for 4 minutes; then nitrogen gas was introduced at 20 sccm, and the bias and current were not changed, and the CrN layer was deposited for 4 minutes.

[0077] (3) Close the gas valve to lower the chamber temperature to room temperature (in the present invention, room temperature refers to 15-30°C, the same below), introduce 55 sccm of argon, and apply a pulsed negative bias of 200 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 100 W; use DC sputtering to sputter the C target with a current of 3.0 A and a deposition time of 50 min.

[0078] Through the above steps, a 402.8 nm composite coating was obtained on the surface of the stainless steel substrate. The Cr atomic percentage of the coating surface was 2.15 at.%, and the C atomic percentage was 86.24 at.%. The XRD spectrum is shown in FIG. Figure 1 As shown, the above doping structure is confirmed.

[0079] It should be noted that in addition to Cr and C, there are also small amounts of O (10.54 at.%) and N (1.07 at.%) on the surface of the film. The N element comes from the nitrogen remaining in the cavity during the coating preparation process, and the O element comes from the oxygen adsorbed on the surface of the coating when it is exposed to the air. For example, oxygen has a higher electronegativity than nitrogen and is more active. It is more easily adsorbed on the surface in the air and forms bonds with the C in the coating for oxidation. Therefore, the sum of the above-mentioned Cr and C element percentages is not equal to 100%.

[0080] The above structural parts were subjected to tribological tests, especially the friction test with the polymer pair. Specifically, the test was carried out under dry friction conditions of load 5N, frequency 2Hz, and distance 5mm, and the test was carried out with a PEEK ball of 6mm diameter for 120min. The results are shown in the figure below. Figure 2 As shown, the friction coefficient is 0.12 and the running-in period is 30 minutes.

[0081] Example 2

[0082] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0083] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum chamber with a degree of less than 4*10 -5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0084] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and the Cr layer was deposited for 4 minutes; then nitrogen gas was introduced at 20 sccm, and the bias and current were not changed, and the CrN layer was deposited for 4 minutes.

[0085] (3) Close the gas valve to lower the chamber temperature to room temperature, introduce argon at 55 sccm, and apply a pulsed negative bias of 200 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 200 W; use DC sputtering to sputter the C target with a current of 3.0 A and a deposition time of 50 min.

[0086] Through the above steps, a 417.5 nm composite coating was obtained on the surface of the stainless steel substrate. The atomic percentage of Cr on the coating surface was 3.73 at.%, and the atomic percentage of C was 80.14 at.%.

[0087] Tribological tests were performed on the above-mentioned structural parts, especially the friction tests with the polymer pairings. Specifically, the parts were ground against a PEEK ball with a diameter of 6 mm for 120 minutes under dry friction conditions of a load of 5 N, a frequency of 2 Hz, and a distance of 5 mm. The friction coefficient was 0.2 and the running-in period was 80 minutes.

[0088] Example 3

[0089] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0090] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum chamber with a degree of less than 4*10 -5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0091] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and the Cr layer was deposited for 4 minutes; then nitrogen gas was introduced at 20 sccm, and the bias and current were not changed, and the CrN layer was deposited for 4 minutes.

[0092] (3) Close the gas valve to lower the chamber temperature to room temperature, introduce argon at 55 sccm, and apply a pulsed negative bias of 200 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 300 W; use DC sputtering to sputter the C target with a current of 3.0 A and a deposition time of 40 min.

[0093] Through the above steps, a 398.5 nm composite coating was obtained on the surface of the stainless steel substrate, and the atomic percentage of Cr on the coating surface was 6.63 at.%, and the atomic percentage of C was 79.74 at.%.

[0094] Tribological tests were performed on the above-mentioned structural parts, especially the friction tests with the polymer pairings. Specifically, the parts were ground against a PEEK ball with a diameter of 6 mm for 120 minutes under dry friction conditions of a load of 5 N, a frequency of 2 Hz, and a distance of 5 mm. The friction coefficient was 0.5 and the running-in period was 65 minutes.

[0095] Example 4

[0096] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0097] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum chamber with a degree of less than 4*10 -5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0098] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and a Cr layer was deposited for 4 minutes; then nitrogen gas was introduced for 20 seconds, and the bias and current were not changed, and a CrN layer was deposited for 4 minutes.

[0099] (3) Close the gas valve to lower the chamber temperature to room temperature, introduce argon at 55 sccm, and apply a pulsed negative bias of 200 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 400 W; use DC sputtering to sputter the C target with a current of 3.0 A and a deposition time of 30 min.

[0100] Through the above steps, a 410.5 nm thick composite coating was obtained on the surface of the stainless steel substrate. The atomic percentage of Cr on the coating surface was 15.52 at.%, and the atomic percentage of C was 70.85 at.%.

[0101] Tribological tests were performed on the above-mentioned structural parts, especially the friction tests with the polymer pairing. Specifically, the parts were ground against a PEEK ball with a diameter of 6 mm for 120 minutes under dry friction conditions of a load of 5 N, a frequency of 2 Hz, and a distance of 5 mm. The friction coefficient was 0.38 and the running-in period was 35 minutes.

[0102] Example 5

[0103] This embodiment illustrates the test of the abrasion resistance of the composite coating / structure prepared in Example 1 and other polymers, as shown below:

[0104] The PEEK balls with a diameter of 6 mm in Example 1 were replaced with PTFE balls of the same size, and the running and grinding test was carried out using the same method. The friction coefficient was 0.16 and the running-in period was 4 minutes.

[0105] The PEEK balls with a diameter of 6 mm in Example 1 were replaced with PI balls of the same size, and the running and grinding test was carried out using the same method. The friction coefficient was 0.19 and the running-in period was 3 minutes.

[0106] The PEEK balls with a diameter of 6 mm in Example 1 were replaced with PSS balls of the same size, and the running and grinding test was carried out using the same method. The friction coefficient was 0.15 and the running-in period was 8 minutes.

[0107] The curve diagram of the above friction test is as follows: Figure 3 shown.

[0108] It should be noted that the technical solution provided by the present invention is not only applicable to the range of matching material selection exemplified in the above embodiments, but also common polymers that can produce self-adhesive chemical reactions can be applied to the above composite coating and achieve better technical effects than before doping.

[0109] Example 6

[0110] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, which is substantially the same as that of Example 1, except that the specific parameters in step (2) and step (3) are different, as shown below:

[0111] (2) The chamber temperature was heated to 130°C, argon gas was introduced at 45 sccm, a pulsed negative bias voltage of 80 V and a current of 3 A were applied, and a Cr layer was deposited for 5 minutes; then nitrogen gas was introduced at 15 sccm, and the bias voltage and current were not changed, and a CrN layer was deposited for 5 minutes.

[0112] (3) Close the gas valve to lower the chamber temperature to room temperature, introduce 45 sccm of argon, and apply a pulsed negative bias of 180 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 100 W; use DC sputtering to sputter the C target with a current of 2.5 A and a deposition time of 50 min.

[0113] The friction structure prepared in this embodiment has the same level of running-in performance as that of Example 1, and its running-in time and friction coefficient are significantly reduced compared with the film layer not doped with Cr.

[0114] Example 7

[0115] This embodiment provides a metal-doped carbon-based composite coating / structure and a preparation method thereof, which is substantially the same as that of Example 1, except that the specific parameters in step (2) and step (3) are different, as shown below:

[0116] (2) The chamber temperature was heated to 170°C, argon gas was introduced at 65 sccm, a pulsed negative bias of 120 V and a current of 4 A were applied, and the Cr layer was deposited for 10 minutes; then nitrogen gas was introduced at 25 sccm, and the bias and current were not changed, and the CrN layer was deposited for 10 minutes.

[0117] (3) Close the gas valve to lower the chamber temperature to room temperature, introduce argon gas at 65 sccm, and apply a pulsed negative bias of 220 V; use HiPIMS technology to sputter the Cr target with a sputtering power of 400 W; use DC sputtering to sputter the C target with a current of 3.5 A and a deposition time of 30 min.

[0118] The friction structure prepared in this embodiment has the same level of running-in performance as that of Example 1, and its running-in time and friction coefficient are significantly reduced compared with the film layer not doped with Cr.

[0119] Comparative Example 1

[0120] This embodiment provides a pure carbon-based composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0121] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum chamber with a degree of less than 4*10 -5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0122] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and the Cr layer was deposited for 4 minutes; then nitrogen gas was introduced at 20 sccm, and the bias and current were not changed, and the CrN layer was deposited for 4 minutes.

[0123] (3) Close the gas valve, lower the chamber temperature to room temperature, introduce argon gas at 55 sccm, and apply a pulsed negative bias of 200 V; use DC sputtering C target, the current is 3.0 A, and the deposition time is 50 min.

[0124] Through the above steps, a 447.9 nm composite coating was obtained on the surface of the stainless steel substrate, and the atomic percentage of Cr on the coating surface was 0 at.%.

[0125] The same test method was used to grind the steel sheet against a PEEK ball with a diameter of 6 mm for 120 minutes under dry friction conditions with a load of 5 N, a frequency of 2 Hz, and a distance of 5 mm. The friction coefficient continued to fluctuate and rose to 0.6 after 120 minutes.

[0126] Compared with the examples, the comparative example has a high friction coefficient and a long friction running-in period. This is mainly because the non-metal-doped amorphous carbon coating undergoes an adhesive chemical reaction with the polymer, which is not conducive to solid lubrication and the stability of the friction coefficient.

[0127] Comparative Example 2

[0128] This embodiment provides a pure chromium composite coating / structure and a preparation method thereof, and the specific steps are as follows:

[0129] (1) First, use anhydrous ethanol and acetone to clean the stainless steel substrate, and then put the cleaned and dried substrate into a vacuum chamber with a degree of less than 4*10 -5 Argon gas at 35 sccm was introduced into the vacuum chamber of 1.8 mTorr. When the chamber pressure reached 1.8 mTorr, a 200 V pulsed negative bias was applied to the stainless steel substrate, and the etching time was 40 min.

[0130] (2) The chamber temperature was heated to 150°C, argon gas was introduced at 55 sccm, a pulsed negative bias of 100 V and a current of 3.5 A was applied, and the Cr layer was deposited for 4 minutes; then nitrogen gas was introduced at 20 sccm, and the bias and current were not changed, and the CrN layer was deposited for 4 minutes.

[0131] (3) Close the gas valve, lower the chamber temperature to room temperature, introduce argon at 55 sccm, and apply a pulsed negative bias of 200 V; use HIPIMS to sputter the Cr target with a sputtering power of 1800 W and a deposition time of 4 min.

[0132] Through the above steps, a composite coating with a thickness of 422.1 nm was obtained on the surface of the stainless steel substrate, and the atomic percentage of C on the coating surface was 0 at.%.

[0133] Using the same test method, under dry friction conditions of load 5N, frequency 2Hz, and distance 5mm, it was ground against a PEEK ball with a diameter of 6mm for 120 minutes. The friction coefficient was 0.7 in the first 60 minutes and 0.73 after 60 minutes.

[0134] Compared with the examples, the friction coefficient of the comparative example is very high. This is mainly because the pure metal coating lacks a solid lubricating phase and will cause severe abrasive wear when rubbing against the polymer pair.

[0135] Comparative Example 3

[0136] This embodiment provides a chromium-doped composite coating / structure and a preparation method thereof, which is substantially the same as the embodiment, with the main differences being:

[0137] In step (3), a direct current power supply (DCMS) was used to sputter the C target and the Cr target, while HiPIMS was not used to sputter the Cr target. By adjusting the sputtering parameters, a carbon-based film with the same elemental composition ratio and the same thickness as in Example 1 was obtained.

[0138] The surface morphology of the structural parts obtained in this comparative example was characterized and compared with that of Example 1. Figure 4a and Figure 4b As shown, the coating obtained in this comparative example has poor surface density. This is because the DC power supply has a low ionization rate on the target material, which cannot produce a highly ionized plasma. As a result, the columnar crystals in the deposited transition layer are large in size, affecting the surface density and making it unnecessary to perform friction testing on it.

[0139] Comparative Example 4

[0140] This embodiment provides a chromium-doped composite coating / structure and a preparation method thereof, which is substantially the same as the embodiment, with the main differences being:

[0141] In step (2), only the Cr transition layer is sputtered or no transition layer is provided, and by adjusting the sputtering parameters, a carbon-based film having the same element composition ratio and the same thickness as that of Example 1 is obtained.

[0142] The bonding strength test of the structural parts obtained in this comparative example is compared with the results of Example 1. Figure 5 As shown, the coating obtained in this example was found to have poor adhesion. The main reason is that the hardness difference between the metal and the carbon-based coating is large (the hardness of the amorphous carbon coating can reach 15-35GPa), resulting in an "eggshell effect" and interface mismatch problems, which can easily lead to coating damage, making it meaningless to conduct friction tests and obtain relevant data.

[0143] Comparative Example 5

[0144] This embodiment provides a chromium-doped composite coating / structure and a preparation method thereof, which is substantially the same as the embodiment, with the main differences being:

[0145] In step (3), a magnetic filtered cathode arc is used to deposit a carbon-based coating, as shown below.

[0146] (3) Start the pulsed cathode arc evaporation device, set the pulse frequency to 10 Hz, and evaporate the Cr-doped carbon-based film for 3 minutes.

[0147] Using the same test method, under dry friction conditions of a load of 5N, a frequency of 2Hz, and a distance of 5mm, it was ground against a PEEK ball with a diameter of 6mm for 60min. The friction coefficient was 0.6 and the friction running-in period was 8min. It should be noted that although the running-in period is short, this is due to the large friction coefficient that it can ultimately achieve. Continuing to extend the running-in time cannot produce a gradual decrease in the friction coefficient similar to the running-in curve of Example 1, and does not mean that the running-in speed of this comparative example is better.

[0148] Compared with the examples, the friction coefficient of the comparative example is very high, which is mainly due to the high sp 3 The carbon bond content makes it difficult to form a graphitized solid lubricating phase, and the synergistic effect between the chromium doping and the amorphous carbon layer mentioned above cannot be produced. Severe fatigue wear will occur when rubbing against the polymer pair.

[0149] Based on the above embodiments and comparative examples, it can be clearly seen that:

[0150] (1) The embodiment of the present invention optimizes the content of doped metal elements and regulates the friction interface between the coating and the polymer. The appropriate Cr content can maintain the excellent lubricity of the carbon-based coating without affecting the formation process of the amorphous carbon graphitized friction film. At the same time, it can inhibit the free radicals such as ROC·, RO·, RC· formed after the friction on the polymer surface from reacting with the C on the amorphous carbon surface to form a lubricating interface between the metal and the amorphous carbon, shorten the friction running-in period of the pair, reduce the friction coefficient, and increase the potential for the pair to be applied in other fields.

[0151] (2) The embodiment of the present invention combines high-power pulsed magnetron sputtering and DC magnetron sputtering technology to deposit void-free, high-density coatings at low substrate temperatures. The operating environment is safe and the process is simple and easy to control, which is conducive to industrial production applications.

[0152] It should be understood that the above embodiments are merely illustrative of the technical concepts and features of the present invention. Their purpose is to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. They are not intended to limit the scope of protection of the present invention. Any equivalent variations or modifications made in accordance with the spirit and substance of the present invention are intended to be encompassed within the scope of protection of the present invention.

Claims

1. A friction pair, characterized in that: It comprises a friction structure and a friction body which frictionally cooperates with the friction structure, wherein the friction body is made of pure PEEK on the friction surface; The friction structure comprises a substrate and a composite coating arranged on a friction surface of the substrate, wherein the composite coating comprises a transition layer and an amorphous carbon layer stacked in sequence in a direction away from the substrate, and the amorphous carbon layer is doped with Cr; The amorphous carbon layer is formed of a hydrogen-free amorphous carbon material formed by mixing a diamond phase and a graphite phase, the molar ratio of the diamond phase to the graphite phase in the amorphous carbon layer is 1:2-1:5, and the atomic percentage of Cr in the amorphous carbon layer is 2.15-15.52%; The preparation method of the composite coating comprises: Using magnetron sputtering, a Cr layer and a CrN layer are sequentially deposited on the surface of the substrate to form the transition layer; A C target material is sputtered by direct current magnetron sputtering, and a Cr target material is sputtered by pulsed magnetron sputtering at the same time, and the amorphous carbon layer is co-deposited on the surface of the CrN layer. When depositing the amorphous carbon layer, the Ar flow rate is 45-65 sccm, the pulsed negative bias voltage is 180-220 V, the direct current is 2.5-3.5 A, the power of the pulsed magnetron sputtering is 100-400 W, and the deposition time is 30-50 min.

2. The friction pair according to claim 1, characterized in that: The thickness of the composite coating is 300-500 nm, and the thickness of the transition layer is 150-240 nm.

3. The friction pair according to claim 2, characterized in that: The transition layer comprises a Cr layer and a CrN layer which are sequentially stacked in a direction away from the substrate, the thickness of the Cr layer is 80-120 nm, the thickness of the CrN layer is 80-120 nm, and the thickness of the amorphous carbon layer is 150-300 nm.

4. The friction pair according to claim 1, characterized in that: The sputtering method of the Cr layer and the CrN layer is selected from DC magnetron sputtering. Before the magnetron sputtering, the substrate is cleaned and etched.

5. The friction pair according to claim 4, characterized in that: The CrN layer is deposited by introducing a nitrogen source on the basis of magnetron sputtering of the Cr layer; The nitrogen source includes nitrogen gas, the Ar flow rate during the deposition of the Cr layer and the CrN layer is 45-65 sccm, the pulse negative bias voltage is 80-120 V, the chamber pressure is 2.0-2.5 mTorr, the chamber temperature is 130-170° C., and the deposition time is 5-10 min; The N2 flow rate when depositing the CrN layer is 15-25 sccm.

6. The friction pair according to claim 1, characterized in that: The friction pair is a dry friction pair.

7. The friction pair according to claim 1, characterized in that: The running-in period of the friction pair is less than 30 minutes. After the running-in period, the friction coefficient of the friction pair is less than 0.

2.

8. Use of the friction pair according to any one of claims 1 to 7 in the field of mechanical seals.