A low-density cement slurry for cementing and preparation method thereof

By using a high water-to-solid ratio and deep activation technology, combined with fly ash, slag and microsilica, and using calcined gypsum and strong acid-weak alkaline salt activators, a network structure is formed, which solves the problem of insufficient density and poor pressure resistance of low-density cement slurry in Changqing oil and gas field, and achieves low-cost, high-strength cement slurry sealing effect.

CN116262656BActive Publication Date: 2024-11-15CHINA NAT PETROLEUM CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202111529222.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-15
Publication Date
2024-11-15
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

Existing low-density cement slurry in the Changqing oil and gas field has problems such as insufficient density, poor pressure resistance, and high cost. In particular, when using expensive cenospheres and glass microspheres, increasing the water-to-solid ratio to reduce density leads to decreased strength and increased water separation.

Method used

Employing a high water-to-solid ratio, deep activation, and stabilization system, fly ash, slag, and silica fume are mixed with oil well cement, and calcined gypsum and strong acid-weak alkaline inorganic salt activators are added to form a network structure, controlling the hydration reaction rate and ensuring the stability and strength of the low-density cement slurry.

Benefits of technology

While reducing density, it ensures the structural stability and strength of the cement slurry, has good pressure resistance, moderate cost, and is suitable for sealing oil and gas wells at 45-85℃. The density increase is ≤0.03 g/cm3, meeting the construction requirements of Changqing Oil and Gas Field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116262656B_ABST
    Figure CN116262656B_ABST
Patent Text Reader

Abstract

The present invention provides a low-density cement slurry for cementing and a preparation method thereof. The low-density cement slurry for cementing comprises the following components in parts by weight: 25-30 parts of oil well cement, 35-45 parts of fly ash, 20-30 parts of slag, 5-10 parts of microsilica powder, 2-5 parts of stabilizer, 2-4 parts of activator, 1-2.5 parts of fluid loss reducer, 0.05-0.2 parts of retarder, and 115-150 parts of water. The present invention utilizes the rapid adsorption of gypsum, microsilica powder and G-grade oil well cement with water to form a network structure, which binds and supports fly ash and slag powder particles. In the later stage, after a certain period of infiltration, swelling and cracking, the fly ash and slag powder particles are more likely to expand the active bonds in the deep layer of the particles that can participate in the hydration reaction, bind and combine more free water to participate in the hydration reaction of the structure, and ensure the structural stability of the low-density cement slurry and the non-collapse and non-shrinkage of the solid volume.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum cementing engineering, and in particular relates to a low-density cement slurry for cementing and a preparation method thereof. Background Art

[0002] Well cementing is the process of injecting cement slurry between the open hole formation and the casing. When the cement slurry solidifies, it seals and separates the formation and supports and protects the casing. Due to the limitations of formation conditions, low-density cement slurry is often used to fill the non-producing layers in the middle and upper parts of the wellbore to avoid fracturing the formation due to high system density, causing cement slurry to leak into the formation, reducing the length of the cement filling section in the annulus and affecting the cementing quality of the entire well.

[0003] The existing low-density cement slurry system generally uses lightening materials and increases the water-cement ratio to reduce the system density. Due to the constraints of the lightening material performance, different lightening fillers (fly ash, plate soil, slag, kaolin, floating beads, glass beads and glazed expanded perlite, etc.) are used. Therefore, the low-density system has different density ranges and performance characteristics. Especially in the Changqing oil and gas fields in the "three lows" area, the low-density system density is generally required to be less than 1.35g / cm 3 , the lightening materials mostly use low-density floating beads, glass beads and glazed expanded perlite. The first two of the above materials have good pressure resistance, but the price is high, and the system cost has remained high; the latter, although moderately priced, lacks pressure resistance, the underground system is compressed, and the density is significantly increased, which is easy to cause leakage and reduced sealing section. Fly ash that can fully withstand pressure (2.3-2.8 g / cm 3 )、Slate(2.6-2.9 g / cm 3 )、Slag(2.6-2.9 g / cm 3 The stable cement slurry system formed by mixing granular materials such as ) with cement has a density of 1.45-1.55 g / cm 3 This density cannot meet the cementing requirements of the leaky strata in the Changqing area; reducing the density by increasing the water-to-solid ratio results in a significant decrease in strength, while the amount of water separation increases and the volume shrinks, making it impossible to meet the requirements of the construction stratum conditions.

[0004] On March 8, 2019, the State Intellectual Property Office published an invention patent with the publication number CN109437710A, and the patent name is a high water-cement ratio, low-cost, low-density cementing cement slurry. The patent consists of oil well cement, fly ash, microsilica powder, early strength agent, ternary activator and fluid loss reducer, dispersant, defoamer and water. The activator is a mixture of soda lime and magnesium carbonate. Although the water-solid ratio reaches 1.25-1.4, the use of inorganic salt early strength agent is not conducive to deep activation. The density range is 1.30-1.35 g / cm 3 . Summary of the invention

[0005] The purpose of the present invention is to provide a low-density cement slurry for cementing, which overcomes the above-mentioned technical problems existing in the prior art.

[0006] Another object of the present invention is to provide a method for preparing low-density cement slurry for cementing, which adopts high water-solid ratio, deep activation and stabilization system technology to solve the difficult problems existing in existing cementing work.

[0007] To this end, the technical solution provided by the present invention is as follows:

[0008] A low-density cement slurry for well cementing comprises the following components in parts by weight: 25-30 parts of oil well cement, 35-45 parts of fly ash, 20-30 parts of slag, 5-10 parts of microsilica powder, 2-5 parts of stabilizer, 2-4 parts of activator, 1-2.5 parts of fluid loss reducer, 0.05-0.2 parts of retarder and 115-150 parts of water.

[0009] The particle size of the microsilica powder is 0.5-10 μm, and the silicon oxide content is greater than 92%.

[0010] The stabilizer is gypsum with a particle size of less than 200 μm, CaSO 4 · 1 / 2 H 2 O content is greater than 90%.

[0011] The activator is MgSO 4 、Al 2 (SO 4 ) 3 ,AlCL 3 A mixture with a mass ratio of 2:0.8-1.2: 0.8-1.2.

[0012] The oil well cement is G-grade oil well cement, the fly ash is secondary fly ash, and the slag is S105-grade slag.

[0013] The density of cement slurry is 1.25-1.35g / cm 3 .

[0014] A method for preparing low-density cement slurry for cementing comprises the following steps:

[0015] Step 1) mixing and stirring the formulated amount of oil well cement, fly ash, slag, microsilica powder, stabilizer and activator to obtain a dry mix;

[0016] Step 2) mixing and stirring the fluid loss reducer, retarder and water in the formula amount to obtain slurry water;

[0017] Step 3) Add the dry mix into the slurry preparation water, mix and stir evenly to obtain cement slurry.

[0018] The beneficial effects of the present invention are:

[0019] The low-density cement slurry for cementing provided by the present invention does not use hollow lightening materials with an upper pressure resistance limit. It solves the technical problems existing in existing cementing work by mixing low-cost fly ash, slag powder and microsilica powder with oil well cement, and adopts high water-solid ratio, deep activation and stabilization system technology.

[0020] The present invention utilizes the rapid adsorption of gypsum, microsilica powder and G-grade oil well cement with water to form a mesh structure, which binds and supports the fly ash and slag powder particles. In the later stage, the fly ash and slag powder particles undergo a certain period of infiltration, swelling and cracking, and a larger amount of active bonds deep in the particles that can participate in the hydration reaction are unfolded, and more free water is bound and combined to participate in the hydration reaction of the structure, ensuring the structural stability of the low-density cement slurry and the non-collapse and non-shrinkage of the solid volume. Compared with the prior art, the present invention can increase the ratio of liquid phase water to solid phase material from 0.8-1.0 to 1.1-1.55, while reducing the density of the system, ensuring that the system is not stratified, the water separation does not exceed the standard, and the system does not shrink or collapse when solidified.

[0021] The present invention adopts strong acid weak alkaline inorganic salt MgSO 4 、Al 2 (SO 4 ) 3 ,AlCL 3 As an activator to control the hydration reaction rate, the overall alkalinity of the system can be appropriately reduced in advance to restrict the early hydration rate of the hydraulic material, so that the fly ash and slag particles with a hydration rate lower than that of cement can swell and crack better, so that more active glass chemical bonds inside can participate in the subsequent hydration reaction, and more liquid water can be combined to participate in the CSH structure to achieve the standard of system strength. In the above reaction process, as the hydration reaction proceeds slowly, H + Ions gradually join the hydration structure, OH - The ions gradually increase, and the fly ash and slag particles, which account for the majority, form cracking. At this time, the increase in alkalinity can accelerate and deepen the hydration reaction and activate the fly ash and slag more deeply.

[0022] The low-density cement slurry provided by the present invention can be used for sealing non-producing layers of various oil and gas wells. The use temperature range is 45-85°C, the bonding strength is ≥3.5 / 7.0MPa (curing conditions: 45°C / normal pressure / 24h / 48h, which is higher than the specified value of the low-density system in the petroleum industry standard), and the pressure resistance performance is: the density increase value is ≤0.03 g / cm 3(Pressure method: high temperature and high pressure thickener 40MPa / 80℃ / 30min / 30min), the system has good stability and low friction resistance in cementing construction; the material price is moderate, there are no special requirements for mixing, transportation and use, and it has high versatility.

[0023] The following will provide a further detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the cement slurry thickening test curve of Example 1 of the present invention;

[0025] Figure 2 This is the cement slurry thickening test curve of Example 3 of the present invention. DETAILED DESCRIPTION

[0026] The following describes the implementation of the present invention through specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0027] The exemplary embodiments of the present invention are now described with reference to the accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. These embodiments are provided to disclose the present invention in detail and completely and to fully convey the scope of the present invention to those skilled in the art. The terms used in the exemplary embodiments are not intended to limit the present invention.

[0028] The invention provides a low-density cement slurry for well cementing, comprising the following components in parts by weight: 25-30 parts of oil well cement, 35-45 parts of fly ash, 20-30 parts of slag, 5-10 parts of microsilica powder, 2-5 parts of stabilizer, 2-4 parts of activator, 1-2.5 parts of fluid loss reducer, 0.05-0.2 parts of retarder and 115-150 parts of water.

[0029] The particle size of the microsilica powder is 0.5-10 μm, and the silicon oxide content is greater than 92%.

[0030] The stabilizer is gypsum with a particle size of less than 200 μm, CaSO 4 · 1 / 2 H 2 O content is greater than 90%.

[0031] The activator is MgSO 4 、Al 2 (SO 4 ) 3 ,AlCL 3 A mixture with a mass ratio of 2:0.8-1.2: 0.8-1.2.

[0032] The oil well cement is G-grade oil well cement, the fly ash is secondary fly ash, and the slag is S105-grade slag. G-grade oil well cement mixed with admixtures and external additives is suitable for most cementing operations, and can be prepared with low-density materials to prepare a low-density cement slurry system for sealing low-pressure and easily exposed formations. Secondary fly ash has a 45μm square hole sieve residue of no more than 25%, and its particle size is generally between 1-100μm, and its fineness is smaller than that of primary fly ash, but the water demand of secondary fly ash is greater than that of primary fly ash. This application adopts an increased water-solid ratio, so secondary fly ash is preferred. The content of active calcium, silicon, aluminum and other inorganic substances in S105-grade slag is greater than 30%, which can increase the water consumption, and the fluidity meets the standard after addition.

[0033] The density of cement slurry is 1.25-1.35g / cm 3 .

[0034] Embodiment 1:

[0035] The present embodiment provides a low-density cement slurry for cementing, comprising the following components in parts by weight: 30 parts of oil well cement, 35 parts of fly ash, 20 parts of slag, 5 parts of microsilica powder, 3 parts of stabilizer, 2.5 parts of activator, 2.5 parts of fluid loss reducer, 0.1 parts of retarder, and 125 parts of water.

[0036] In this embodiment, the oil well cement is G-grade oil well cement; the fly ash is secondary fly ash; the slag is S105-grade slag; and the activator is MgSO 4 :Al 2 (SO 4 ) 3 :AlCL 3 =2:1:1 (mass ratio); the fluid loss reducer is polyvinyl alcohol (GJ-S), which is polyvinyl alcohol 1778 fluid loss reducer produced by Good Company, or other polyvinyl alcohol 1788 products that meet the standards of the petroleum industry. The amount of water loss in the system can be controlled to be less than 200ml; the retarder is starch retarder GH-3 purchased from Good Company. Other similar products that meet the standards of the petroleum industry and whose thickening time can be controlled within the range that meets the requirements of the construction conditions are acceptable.

[0037] Principle of the invention:

[0038] Under the condition that the main materials are similar, the lower the density, the higher the water consumption, and the more difficult it is to stabilize the system. It is necessary to add a stabilizer to improve the stability of the system. The existing technology (such as publication numbers CN103725277A, CN101475347A and CN109437710A) mainly relies on microsilica powder to increase viscosity to maintain the stability of the system. The difference between the present invention and the existing technology is that not only microsilica powder is used to increase viscosity, but also strong acid and weak alkaline inorganic salts are used to deeply activate fly ash and slag, and gypsum that can quickly bind water molecules to form a network structure is also added to better stabilize the system and prevent the system from settling and stratification.

[0039] Reducing the system density increases the amount of water in the system, which cannot react with cement, fly ash and other cementitious materials for hydration, resulting in an increase in the amount of solid free water, which will reduce the bonding strength of the system and affect the strength of the cement stone, which does not meet the construction requirements. The present invention does not adopt the early strength route of strong electrolytes and alkaline admixtures in the prior art patents that quickly combine with materials for hydration, but instead adopts a method of controlling the hydration speed. In a neutral and weakly acidic system solution, a certain amount of swelling first occurs in the aqueous solution to ensure that more chemical bonds inside the particles can participate in the later hydration reaction, thereby reducing the amount of free water, increasing the reaction depth, and increasing the strength of the system.

[0040] Among them, strong acid and weak alkaline inorganic salts are used as activators to control the hydration reaction type. The overall alkalinity of the system is appropriately reduced in advance, which can restrict the early hydration rate, facilitate the fly ash and slag particles with higher inertness, and can swell and crack better, so that more active glass inside can participate in the subsequent hydration reaction, combine more liquid water to participate in the CSH structure, and achieve the strength of the system. During the above reaction process, as the hydration reaction proceeds slowly, H+ ions gradually participate in the hydration structure, OH- ions gradually increase, and at the same time, the fly ash and slag particles that account for the majority of the formation of cracks. At this time, the increase in alkalinity can accelerate and deepen the hydration reaction, and activate the fly ash and slag more deeply. However, the existing technology uses alkaline activation, which quickly reacts on the surface of the particles, the total alkalinity increases rapidly, and a covering film is formed on the surface of the particles, which inhibits the subsequent hydration reaction and cannot combine more free water, resulting in increased water precipitation in the system and substandard strength.

[0041] Using architectural plaster, CaSO 4 · 1 / 2 H 2 O content greater than 90%, particle size less than 200μm

[0042] The method for preparing low-density cement slurry for cementing of the present invention comprises the following steps:

[0043] Step 1) mixing and stirring the formulated amount of oil well cement, fly ash, slag, microsilica powder, stabilizer and activator to obtain a dry mix;

[0044] Step 2) mixing and stirring the fluid loss reducer, retarder and water in the formula amount to obtain slurry water;

[0045] Step 3) Add the dry mix into the slurry preparation water, mix and stir evenly to obtain cement slurry.

[0046] The density of the low-density cement slurry prepared in this example is 1.35 g / cm 3 .

[0047] Embodiment 2:

[0048] The present embodiment provides a low-density cement slurry for cementing, comprising the following components in parts by weight: 25 parts of oil well cement, 45 parts of fly ash, 20 parts of slag, 10 parts of microsilica powder, 4 parts of stabilizer, 3.5 parts of activator, 2.5 parts of fluid loss reducer, 0.1 part of retarder, and 137 parts of water.

[0049] In this embodiment, the oil well cement is G-grade oil well cement; the fly ash is secondary fly ash; the slag is S105-grade slag; and the activator is MgSO 4 :Al 2 (SO 4 ) 3 :AlCL 3 =2:0.8:0.8 (mass ratio); the fluid loss reducer is polyvinyl alcohol (GJ-S), which is polyvinyl alcohol 1778 type fluid loss reducer produced by Good Company, or other polyvinyl alcohol 1788 type products that meet the standards of the petroleum industry. The amount of water loss in the system can be controlled to be less than 200ml; the retarder is starch retarder GH-3 purchased from Good Company. Other similar products that meet the standards of the petroleum industry and whose thickening time can be controlled within the range that meets the requirements of the construction conditions are acceptable.

[0050] The preparation method is the same as that of Example 1.

[0051] The density of the low-density cement slurry prepared in this example is 1.30 g / cm 3 .

[0052] Embodiment 3:

[0053] The present embodiment provides a low-density cement slurry for cementing, comprising the following components in parts by weight: 25 parts of oil well cement, 45 parts of fly ash, 20 parts of slag, 10 parts of microsilica powder, 4.5 parts of stabilizer, 4 parts of activator, 2.5 parts of fluid loss reducer, 0.15 parts of retarder, and 150 parts of water.

[0054] In this embodiment, the oil well cement is G-grade oil well cement; the fly ash is secondary fly ash; the slag is S105-grade slag; and the activator is MgSO 4 :Al 2 (SO 4 ) 3 :AlCL 3 =2:1.2: 1.2 (mass ratio); the fluid loss reducer is polyvinyl alcohol (GJ-S), which is polyvinyl alcohol 1778 type fluid loss reducer produced by Good Company, or other polyvinyl alcohol 1788 type products that meet the standards of the petroleum industry. The amount of water loss in the system can be controlled to be less than 200ml; the retarder is starch retarder GH-3 purchased from Good Company. Other similar products that meet the standards of the petroleum industry and whose thickening time can be controlled within the range that meets the requirements of the construction conditions are acceptable.

[0055] The preparation method is the same as that of Example 1.

[0056] The density of the low-density cement slurry prepared in this example is 1.25 g / cm 3 .

[0057] Embodiment 4:

[0058] This example characterizes the performance of the low-density cement slurry for cementing prepared in Examples 1 to 3.

[0059] 1. Water separation

[0060] According to GB / T10238-2015 Oil Well Cement Section 8. The test results are shown in Table 1. There is a slight visible concave surface after solidification.

[0061] 2. Thickening time

[0062] According to Section 10 of GB / T10238-2015 Oil Well Cement. The experimental conditions are 80℃ / 40MPa / 40min. The test results are shown in Table 1. Figure 1 (Example 1) and Figure 2 (Example 3).

[0063] Table 1 Water analysis results

[0064]

[0065] During the heating process, the cement slurry gradually becomes thermally diluted and the consistency becomes smaller. At 80°C, the consistency is 9-10. Among them, t30 represents the time when the cement slurry reaches a consistency of 30Bc, indicating the start time of the transition from liquid to solid, and is also the upper limit of the safe grouting time; t70 represents the time when the cement slurry reaches a consistency of 70Bc.

[0066] 3. Liquidity

[0067] The test results of Example 1 are shown in Table 2. The test results of Example 2 are shown in Table 3. The test results of Example 3 are shown in Table 4.

[0068] Table 2 Rheological properties of pressure-resistant low-density cement slurry in Example 1 (75 degrees / 30 min / normal pressure)

[0069]

[0070] The test results are as follows: apparent viscosity is 29.5 centipoise, plastic viscosity is 24 centipoise, dynamic shear is 5.5 Pa, rheological index n=0.8596, and consistency coefficient K=0.864.

[0071] Table 3 Rheological properties of pressure-resistant low-density cement slurry in Example 2 (75 degrees / 30 min / normal pressure)

[0072]

[0073] The test results are as follows: apparent viscosity is 25 centipoise, plastic viscosity is 22 centipoise, dynamic shear is 5.0 Pa, rheological index n=0.8456, and consistency coefficient K=0.7713.

[0074] Table 4 Rheological properties of pressure-resistant low-density cement slurry in Example 3 (75 degrees / 30 min / normal pressure)

[0075]

[0076] The test results are as follows: apparent viscosity is 26 centipoise, plastic viscosity is 21 centipoise, dynamic shear is 5.0 Pa, rheological index n is 0.8026, and consistency coefficient K=0.873.

[0077] 4. Maintenance intensity

[0078] According to Section 7 of GB / T119139-2012 Oil Well Cement. The curing conditions are 45℃ and normal pressure. The test results are shown in Table 5.

[0079] Table 5 Curing intensity

[0080]

[0081] 5. Pressure resistance test

[0082] Pressurization method: put the slurry of a certain density into the kettle of the high-temperature and high-pressure thickener, operate the equipment, set the temperature to rise to the bottom hole temperature of 45-80℃ in 25-45min, and at the same time, the pressure rises to 25-40MPa, maintain the above temperature and pressure for 30min, then stop the operation program, reduce the temperature and pressure, take out the slurry, measure the density value, subtract the original density, and obtain the density increase.

[0083] The experimental results show that the density increase after pressure resistance is ≤0.03 g / cm 3 .

[0084] 6. Comparative experiment

[0085] Take the invention patent of CN109437710A, published by the State Intellectual Property Office on March 8, 2019, and the patent name is a high water-cement ratio, low-cost, low-density cementing cement slurry, as a comparative example. The high water-cement ratio, low-cost, low-density cementing cement slurry disclosed in the comparative example is composed of the following raw materials in parts by weight: 40-100 parts of oil well cement, 25-60 parts of fly ash, 30-40 parts of microsilica powder, 2-3 parts of early strength agent, 2-8 parts of ternary activator, 3-3.5 parts of fluid loss reducer, 0-0.2 parts of dispersant, 0.2 parts of defoamer, and 180-272 parts of clean water, wherein the ternary activator is a mixture of soda lime and magnesium sulfate with a mass ratio of 9:1. The comparison results are shown in Table 6.

[0086] Table 6 Performance comparison

[0087]

[0088] As shown in Table 6, compared with the comparative example, the present invention does not use an early strength agent (i.e., an early strength route that quickly combines with the material for hydration), but controls the hydration speed. In the neutral and weakly acidic system solution, a certain amount of swelling first occurs in the aqueous solution to ensure that more chemical bonds inside the particles can participate in the later hydration reaction, so that the amount of free water becomes less, the reaction depth increases, and the system strength increases. Therefore, while increasing the water-to-solid ratio to meet the low density requirements, it is also strong and reduces the amount of water precipitation. Moreover, in the comparative example with a density of 1.25 g / cm 3 In the case of , the cement slurry in this application has obvious settlement, while the density is 1.15-1.5 g / cm 3 All are stable.

[0089] Except for the comparison case, the density is 1.25-1.35g / cm 3 Under the condition of low density hollow material, the prepared slurry will have obvious rupture and collapse under pressure, because the pressure resistance of hollow material has a certain upper limit, resulting in a significant increase in system density, with a density increase of 0.05-0.15g / cm 3 At the same time, the flow resistance increases significantly, causing great hidden dangers to cement slurry cementing construction.

[0090] The low-density cement slurry system developed by the present invention can be used to seal non-producing layers of various oil and gas wells. The operating temperature range is 45-85°C. The bonding strength is ≥3.5 / 7.0MPa (45°C / normal pressure / 24h / 48h curing). The pressure resistance performance is: the density increase value is ≤0.03 g / cm 3 (40MPa / 80℃ / 30min / 30min), indicating that the density of the system at normal temperature / pressure at the wellhead does not contain hollow lightening materials after the temperature / pressure increase at the bottom of the well, and will not collapse or increase in density; the system has good stability, and the flow friction resistance during cementing construction is low, which is conducive to the pumping back of cement slurry and increases the sealing length of cement slurry.

[0091] The above examples are merely illustrative of the present invention and do not constitute a limitation on the protection scope of the present invention. All designs that are the same or similar to the present invention fall within the protection scope of the present invention.

Claims

1. A low-density cement slurry for cementing, characterized in that: The invention comprises the following components in parts by weight: 25-30 parts of oil well cement, 35-45 parts of fly ash, 20-30 parts of slag, 5-10 parts of microsilica powder, 2-5 parts of stabilizer, 2-4 parts of activator, 1-2.5 parts of fluid loss reducer, 0.05-0.2 parts of retarder, and 115-150 parts of water; The activator is a mixture of MgSO4, Al2(SO4)3, and AlCl3, with a mass ratio of 2:0.8-1.2: 0.8-1.2; and the stabilizer is plaster of Paris.

2. The low-density cement slurry for cementing according to claim 1, characterized in that: The particle size of the microsilica powder is 0.5-10 μm, and the silicon oxide content is greater than 92%.

3. The low-density cement slurry for cementing according to claim 1, characterized in that: The particle size of the plaster of Paris is less than 200 μm, and the CaSO4· 1 / 2 H2 O content is greater than 90%.

4. The low-density cement slurry for cementing according to claim 1, characterized in that: The fly ash is secondary fly ash, and the slag is S105 grade slag.

5. The low-density cement slurry for cementing according to claim 1, characterized in that: The density of cement slurry is 1.25-1.35g / cm 3 .

6. A method for preparing low-density cement slurry for cementing according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1) mixing and stirring the formulated amount of oil well cement, fly ash, slag, microsilica powder, stabilizer and activator to obtain a dry mix; Step 2) mixing and stirring the fluid loss reducer, retarder and water in the formula amount to obtain slurry water; Step 3) Add the dry mix into the slurry preparation water, mix and stir evenly to obtain cement slurry.

Citation Information

Cited By

  • Fly ash composite low-density cement paste as well as preparation method and application thereof

    CN122608334A