Tungsten-nickel-iron component and preparation method

The preparation of tungsten-nickel iron components through additive manufacturing technology, combined with vacuum water quenching and sintering processes, solves the problems of uncontrollable chips and waste of steel in the existing technology, and achieves precise control of chip shape and size and high toughness of the material, improving the quality of the chips, thereby improving the quality of the chips, and improving the quality of the material. The power of explosives and the damage ability of weapons.

CN116275103BActive Publication Date: 2024-11-15ADVANCED FOR MATERIALS & EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310167015.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-25
Publication Date
2024-11-15
Estimated Expiration
2043-02-25

AI Technical Summary

Technical Problem

The shape and size of the existing pre-installed fragment weapons are uncontrollable, resulting in waste of steel and the power of explosives being insufficiently utilized.

Method used

Tungsten-nickel iron powder is used to print and prepare tungsten-nickel iron components through additive manufacturing technology, combined with vacuum water quenching technology, the shape and size of the chip are controlled, and the toughness and density of the material are improved through the sintering and ball milling process.

Benefits of technology

It realizes precise control of the shape and size of the fragment, improves the power of explosives and the toughness of the high-specific gravity alloy components of the material, reduces steel waste, and improves the damage ability of the weapon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116275103B_ABST
    Figure CN116275103B_ABST
Patent Text Reader

Abstract

This invention provides a tungsten-nickel-iron component and its preparation method. The preparation method includes: spreading tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component, printing it to obtain a green blank of the tungsten-nickel-iron component; the tungsten-nickel-iron powder has a solid structure and a particle size of 20-40 micrometers; holding the green blank of the tungsten-nickel-iron component at 1100-1200℃ under vacuum for 3-10 hours, and then cooling it to obtain the tungsten-nickel-iron component. The above preparation method uses coarse-grained tungsten powder, resulting in good alloy toughness; it employs additive manufacturing technology, allowing for controllable fragment shape and size; the integrated structure fully utilizes the explosive power and provides extra space for explosive loading, improving the weapon's destructive capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a tungsten-nickel-iron component and a preparation method thereof. Background Art

[0002] The structure of weapons with pre-set fragments whose shape and size can be controlled is a two-layer steel structure with high-density blocks and spheres. The current structure has defects such as uncontrollable fragments and waste of explosive power due to excess steel. However, by using additive manufacturing technology, the entire structure is made of high-density alloy armor-piercing materials, which not only greatly improves the explosive capacity, but also controls the size and shape of the fragments. Summary of the invention

[0003] The main purpose of the present invention is to provide a tungsten-nickel-iron component and a preparation method to solve the technical problems that the fragments of the current pre-set fragments of weapons are uncontrollable and the excess steel wastes the power of explosives.

[0004] To achieve the above object, the present invention provides a method for preparing a tungsten-nickel-iron component, comprising:

[0005] The tungsten-nickel-iron powder is spread according to the designed shape of the tungsten-nickel-iron component, and printed to obtain a green body of the tungsten-nickel-iron component; the tungsten-nickel-iron powder is a solid structure, and the particle size is 20-40 microns;

[0006] The green body of the tungsten-nickel-iron component is kept at 1100-1200° C. under vacuum for 3-10 hours and then cooled to obtain a tungsten-nickel-iron component.

[0007] Optionally, in the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing:

[0008] The oxygen content in the molding chamber is less than 100ppm and the pressure is maintained at 10-40mbar. The laser power for scanning the entity is 400W, the laser power for scanning the contour is 200W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 1500mm / s, the contour scanning speed is 300mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 700℃.

[0009] Optionally, in the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing:

[0010] A laser beam is used to quickly melt the powder according to the slice shape and scanning path. The preset powder thickness is 30 μm, and the powder supply is set to 3 times the powder thickness. After printing is completed, the tungsten-nickel-iron component is placed in the molding chamber for 3 hours.

[0011] Optionally, the green body of the tungsten-nickel-iron component is kept at 1100-1200° C. under vacuum for 3-10 hours, and the cooling step comprises:

[0012] The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, and evacuated to a vacuum degree of less than 10 -3 Pa, maintain annealing temperature at 1200°C, holding time for 4-5h, and cool with the furnace.

[0013] Optionally, the method for preparing the tungsten-nickel-iron powder comprises:

[0014] Mix tungsten powder, nickel powder and iron powder and grind them to obtain mixed powder; wherein the particle size of the tungsten powder is 20-40 microns, the particle size of the nickel powder is 1-3 microns, and the particle size of the iron powder is 1-3 microns;

[0015] Granulating and pressing the mixed powder to obtain a material body;

[0016] After degreasing the material blank at 800° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod;

[0017] The rod is crushed, and particles with a crushed particle size of 25-53 microns are screened to obtain the tungsten-nickel-iron powder.

[0018] Optionally, in the step of ball-milling the mixed tungsten powder, nickel powder and iron powder, the ball-milling medium is ethanol, and 1-3% paraffin is added to the ethanol; the ball-milling time is 24-48 hours, and the ball-to-material ratio of the ball-milling grinding balls is 4:1, and the material is the sum of the tungsten powder, the nickel powder and the iron powder.

[0019] Optionally, the step of granulating the mixed powder comprises: spray-drying and granulating the mixed powder at a gas temperature of 150-200°C.

[0020] Optionally, the mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa, wherein the material green body is a sphere with a diameter of 20-50 mm or a cube with a width of 20-50 mm.

[0021] The present invention also provides a tungsten-nickel-iron component obtained by the above-mentioned preparation method.

[0022] Optionally, the tungsten-nickel-iron component includes a fragment unit, and the fragment unit has a diameter of 200 mm and a height of 240 mm.

[0023] In the above-mentioned preparation method of tungsten-nickel-iron components, tungsten powder, nickel powder and iron powder are used as raw materials to sinter to obtain rods. During the sintering process, the particle size of the tungsten powder increases to form larger tungsten-nickel-iron powder particles, and the nickel powder and iron powder are melted and coated on the surface of the tungsten-nickel-iron powder particles, and the tungsten-nickel-iron component preparation method is obtained after crushing. The above-mentioned preparation method of tungsten-nickel-iron components uses coarse-grained tungsten powder, and the alloy has good toughness; using additive manufacturing technology, the shape and size of the fragments can be controlled, the integrated structure fully utilizes the power of the explosives and can have extra space to load the explosives, thereby improving the weapon's destructive capability; vacuum water quenching technology further improves the toughness of the tungsten-nickel-iron special-shaped shell. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0025] Figure 1 This is a scanning electron microscope image of a tungsten-nickel-iron powder according to an embodiment of the present application at a magnification of 60x;

[0026] Figure 2 This is a scanning electron microscope image of the tungsten-nickel-iron powder according to one embodiment of the present application at a magnification of 2000x.

[0027] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0030] In addition, in the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0031] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0032] To achieve the above object, the present invention provides a method for preparing a tungsten-nickel-iron component, comprising:

[0033] S100: Spreading tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component, printing, and obtaining a green body of the tungsten-nickel-iron component; the tungsten-nickel-iron powder is a solid structure, and the particle size is 20-40 microns.

[0034] The tungsten nickel iron powder has a tungsten particle size of 35-40 microns, and nickel powder and iron powder are coated on the surface of the spherical tungsten powder particles. When additive manufacturing is performed such as through 3D printing, nickel and iron melt to form a bonding phase layer; therefore, the bonding phase layer of the tungsten nickel iron powder is thick and has good mechanical properties; 3D printing promotes uniform distribution of tungsten particles and good consistency; on this basis, the connection between adjacent tungsten nickel iron powders is between bonding phases rather than between tungsten particles, thereby reducing laser power and thermal stress. Therefore, it is more conducive to 3D printing.

[0035] S200: keeping the green body of the tungsten-nickel-iron component at 1100-1200° C. under vacuum for 3-10 hours, cooling, and obtaining a tungsten-nickel-iron component.

[0036] Optionally, in the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing:

[0037] The oxygen content in the molding chamber is less than 100ppm and the pressure is maintained at 10-40mbar. The laser power for scanning the entity is 400W, the laser power for scanning the contour is 200W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 1500mm / s, the contour scanning speed is 300mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 700℃.

[0038] Optionally, in the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing:

[0039] A laser beam is used to quickly melt the powder according to the slice shape and scanning path. The preset powder thickness is 30 μm, and the powder supply is set to 3 times the powder thickness. After printing is completed, the tungsten-nickel-iron component is placed in the molding chamber for 3 hours.

[0040] Optionally, the green body of the tungsten-nickel-iron component is kept at 1100-1200° C. under vacuum for 3-10 hours, and the cooling step comprises:

[0041] The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, and evacuated to a vacuum degree of less than 10 -3 Pa, maintain annealing temperature at 1200°C, holding time for 4-5h, and cool with the furnace.

[0042] In some embodiments, the method for preparing the tungsten-nickel-iron powder comprises:

[0043] S10: ball-milling tungsten powder, nickel powder and iron powder to obtain mixed powder, wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 1-3 microns, and the particle size of the iron powder is 1-3 microns.

[0044] In this step, 1-3 micron tungsten powder, 1-3 micron nickel powder, and 1-3 micron iron powder can be mixed and ball-milled. During the ball-milling process, the tungsten powder, nickel powder, and iron powder are further crushed to form finer particles, and the tungsten powder, nickel powder, and iron powder are mixed more evenly.

[0045] S20: granulating and pressing the mixed powder to obtain a material body.

[0046] In this step, the mixed powder is granulated to form small particles of mixed powder particles, and then pressed into shape, for example, by grinding or cold isostatic pressing, so that the mixed powder particles form a material body with a certain shape. The material body can be spherical, square, cylindrical, etc., and the specific shape is not limited. The volume of the material body is relatively small, and its maximum three-dimensional size is not too large to facilitate calcination. In some embodiments, the maximum size and minimum size of the material body in three dimensions are similar.

[0047] S30: After degreasing the material blank at 800° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod.

[0048] The melting point of nickel powder is 212°C, the melting point of iron powder is 1538°C, and the melting point of tungsten powder is 3400°C. In this step, during the sintering process, the tungsten grains gradually grow, so the particle size of the tungsten powder gradually increases, forming a relatively regular spherical structure, that is, forming spherical tungsten powder particles.

[0049] The melting points of nickel powder and iron powder are relatively low, forming a molten state and coating the surface of the spherical tungsten powder particles. That is, the rod includes a plurality of spherical tungsten powder particles, and the space between adjacent spherical tungsten powder particles is filled with molten iron and nickel.

[0050] Sintering in hydrogen atmosphere at 1450-1530℃ for 2-4 hours, the sintering degree is good, the melting point of nickel powder and iron powder is relatively low, forming a molten state, covering the surface of spherical tungsten powder particles. That is, the rod includes multiple spherical tungsten powder particles, and the adjacent spherical tungsten powder particles are filled with molten iron and nickel.

[0051] If the temperature is too high and the time is too long, a large amount of tungsten, nickel and iron may melt together, destroying the iron and nickel wrapped around the tungsten particles. The subsequent rods are not easy to break, and the tungsten particles are larger and irregular in shape. If the temperature is too low and the time is too short, the tungsten particles may not grow or may not grow to the target range.

[0052] S40: Powdering the rod to obtain tungsten-nickel-iron powder, wherein the tungsten-nickel-iron powder includes tungsten particles and a metal layer covering the tungsten particles, wherein the metal layer is a nickel and iron metal layer.

[0053] In the above-mentioned method for preparing tungsten-nickel-iron powder for additive manufacturing, tungsten powder, nickel powder and iron powder are used as raw materials to sinter to obtain rods. During the sintering process, the particle size of the tungsten powder increases to form spherical tungsten powder particles with larger particles, and the nickel powder and iron powder are melted and coated on the surface of the spherical tungsten powder particles. In the above-mentioned method for preparing tungsten-nickel-iron powder for additive manufacturing, the tungsten particles are 20-40 microns, the average thickness between the tungsten particles after heat treatment is relatively large, and the toughness of the alloy is good. Therefore, it is suitable for preparing high-toughness and high-density alloy parts.

[0054] In some embodiments, in the mixed powder, the step of powdering the rod material comprises:

[0055] S41: Processing the rod into a target rod that meets the size requirements of a non-transferred arc rotating electrode atomization device; the non-transferred arc rotating electrode atomization device includes an atomization furnace and a plasma gun.

[0056] In this step, since the rod is used as the positive electrode in the non-transferred arc rotating electrode atomization device, the size of the rod needs to meet the corresponding size requirements, such as the rod can be processed into a specification of 70mm in diameter and 300mm in length. The non-transferred arc rotating electrode atomization device includes an atomization furnace and a plasma gun, and its specific structure is not limited. For example, it can be a brushless conductive high-speed plasma rotary atomization powder making device in application number 202110832524.7.

[0057] S42: placing the target rod in the atomizing furnace, wherein the atomizing furnace is provided with a protective gas atmosphere and a vacuum degree of 5×10-3 Pa, temperature is 25~30℃, humidity ≤75%RH.

[0058] In this step, the ambient temperature can be kept at 25-30°C and the ambient humidity can be kept at ≤75%RH. The target rod is placed in the atomizing furnace as the positive electrode, and the protective gas argon is filled in. The atomizing furnace is evacuated to a vacuum degree of 5×10 -3 Pa.

[0059] S43: One end of the target rod is heated and melted under the action of the transferred arc formed by the plasma gun to form an alloy powder; wherein the target rod is rotated at a speed of 25000-30000 r / min, the feed speed is 1.6 mm / s, the current of the plasma gun is 1500 A, and the distance between the plasma gun and the target rod is 15-25 mm.

[0060] In this step, the process parameters are set to start the non-transferred arc rotating electrode atomization (NTA-PREP) equipment. The target bar rotates at a speed of 25,000-30,000 r / min, the target bar feed speed is 1.6 mm / s, and the current of the plasma gun is 1500 A. The plasma gun forms a transferred arc to heat and melt one end of the target bar, so that the alloy droplets after the target bar is melted in the atomization chamber are thrown out under the action of centrifugal force, and the alloy droplets are cooled to form alloy powder under the action of surface tension.

[0061] S44: Maintaining a high pressure of 120 KPa in the atomizing furnace for 4 hours, the alloy powder is cooled in the atomizing furnace to obtain tungsten-nickel-iron powder.

[0062] In this step, after the powder making is completed, the high pressure of 120 KPa is maintained in the atomizing furnace for 4 hours and cooled along with the furnace.

[0063] In some embodiments, the method further comprises: passing the cooled alloy powder through a 200-mesh screen to obtain tungsten-nickel-iron powder. For example, after the powder is cooled, it can be sieved using an ultrasonic vibrating sieve machine and then vacuum packaged.

[0064] In some embodiments, in the mixed powder, the mass percentage of tungsten powder is 93-95%, the mass percentage of nickel powder is 3.5-5%, and the mass percentage of iron powder is 1.5-2.1%.

[0065] In some embodiments, the material blank is degreased at 800° C. and then sintered at 1450-1530° C. in a hydrogen atmosphere for 2-4 hours to obtain a rod.

[0066] In some embodiments, in the step of ball-milling the tungsten powder, nickel powder and iron powder, the ball-milling medium is ethanol, and 1-3% paraffin is added to the ethanol. The ball-milling time is 24-36 hours, the ball-to-material ratio of the ball mill is 4:1, and the material is the sum of the tungsten powder, nickel powder and iron powder.

[0067] According to an embodiment of the present application, the step of granulating the mixed powder comprises: spray drying and granulating the mixed powder at a gas temperature of 150-200°C.

[0068] According to the embodiment of the present application, the mixed powder particles formed by granulation are pressed into a material body under a pressure of 150-200 MPa, and the material body is a sphere with a diameter of 20-50 mm or a block with a width of 20-50 mm.

[0069] According to an embodiment of the present application, the rod is subjected to plasma rotating electrode atomization to obtain tungsten-nickel-iron powder, which comprises:

[0070] The rod is subjected to plasma rotating electrode atomization at 25,000 to 30,000 revolutions to obtain tungsten-nickel-iron powder.

[0071] The present invention also provides a method for preparing a high-toughness tungsten-nickel-iron special-shaped shell, comprising:

[0072] The tungsten-nickel-iron powder obtained by the above-mentioned preparation method is used for powder spreading to print the fragment unit. The fragment unit has a three-layer structure.

[0073] The fragment unit is kept at 1200° C. under vacuum for 4-5 hours and then quenched in water to obtain a fragment unit.

[0074] The fragment units are welded to obtain a high-toughness tungsten-nickel-iron special-shaped shell.

[0075] According to an embodiment of the present application, the fragment unit has a diameter of 200 mm and a height of 240 mm.

[0076] The present invention also provides a high-toughness tungsten-nickel-iron special-shaped shell obtained by the above-mentioned preparation method.

[0077] The technical solution of the present application is described below in conjunction with specific embodiments.

[0078] Example 1

[0079] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 24 microns, the particle size of the nickel powder is 1.5 microns, and the particle size of the iron powder is 1.5 microns. The mixed powder is 93% tungsten + 4.9% nickel + 2.1% iron powder.

[0080] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method and a centrifugal nozzle at a gas temperature of 150-200°C.

[0081] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 150MPa, into small balls or small cubes with a diameter of 20mm.

[0082] S104 sintering: After degreasing the material blank at 800°C, sinter it in a hydrogen atmosphere at 950°C for 2 hours to obtain a rod.

[0083] S105 crushing: The rod is crushed to obtain tungsten-nickel-iron powder with a D50 of 33 microns.

[0084] S106 adopts SLM powder 3D printing:

[0085] (1) Raw material mixing: Add each tungsten-nickel-iron powder into a ball mill and mix for 6 hours;

[0086] (2) The three-dimensional model of the tungsten-nickel-iron component to be formed is sliced, and the preset slice thickness is 15 μm; the scanning path adopts a nine-square grid partition scanning, and the area size is 4*4 mm; the preset deflection angle is 40°.

[0087] (3) Set the laser selective melting process parameters and protect the molding chamber with argon gas, control the oxygen content in the molding chamber to be less than 100ppm and maintain the pressure at 10-40mbar. The laser power for scanning the entity is 400W, the laser power for scanning the contour is 200W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 1500mm / s, the contour scanning speed is 300mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 700℃

[0088] (4) Start printing, use a laser beam to quickly melt the powder according to the slice shape and scanning path, the preset powder thickness is 30 μm, and the powder supply is set to 3 times the powder thickness. After printing is completed, the tungsten-nickel-iron component is placed in the molding chamber for 3 hours.

[0089] (5) The removed tungsten-nickel-iron component is heat treated at 1200° C. and maintained under vacuum for 4 hours to obtain a fragment unit.

[0090] The density of the final tungsten-nickel-iron component can reach 99.6%, and the tensile strength can reach 1382MPa.

[0091] Example 2

[0092] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 32 microns, the particle size of the nickel powder is 2 microns, and the particle size of the iron powder is 2 microns. The mixed powder is 95% tungsten + 3.5% nickel + 1.5% iron powder.

[0093] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method and a centrifugal nozzle at a gas temperature of 150-200°C.

[0094] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 180MPa, into small balls or small cubes with a diameter of 30mm.

[0095] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1200°C for 2-4 hours to obtain a rod.

[0096] S105 crushing: The rod is crushed to obtain tungsten-nickel-iron powder with a D50 of 33 microns.

[0097] S106 adopts SLM powder 3D printing:

[0098] Embodiment 2:

[0099] (1) Raw material mixing: Add each tungsten-nickel-iron powder into a ball mill and mix for 6 hours;

[0100] (2) The three-dimensional model of the tungsten-nickel-iron component to be formed is sliced, and the preset slice thickness is 15 μm; the scanning path adopts a nine-square grid partition scanning, and the area size is 4*4 mm; the preset deflection angle is 40°.

[0101] (3) Set the laser selective melting process parameters and protect the molding chamber with argon gas, control the oxygen content in the molding chamber to be less than 100ppm and maintain the pressure at 10-40mbar. The laser power for scanning the entity is 300W, the laser power for scanning the contour is 150W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 2000mm / s, the contour scanning speed is 350mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 600℃

[0102] The laser power for scanning the entity is 350W, the laser power for scanning the contour is 200W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 1500mm / s, the contour scanning speed is 300mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 700℃

[0103] (4) Start printing, use a laser beam to quickly melt the powder according to the slice shape and scanning path, the preset powder thickness is 30 μm, and the powder supply is set to 2 times the powder thickness. After printing is completed, the tungsten-nickel-iron component is placed in the molding chamber for 3 hours.

[0104] (5) The removed tungsten-nickel-iron component is subjected to heat treatment, wherein the heat treatment process is: 1200° C., maintained under vacuum for 4-5 hours, to obtain a fragment unit;

[0105] The density of the final tungsten-nickel-iron component reaches 98.2%, and the tensile strength can reach 1364MPa.

[0106] Example 3

[0107] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 32 microns, the particle size of the nickel powder is 2 microns, and the particle size of the iron powder is 2 microns. The mixed powder is 95% tungsten + 3.5% nickel + 1.5% iron powder.

[0108] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method and a centrifugal nozzle at a gas temperature of 150-200°C.

[0109] S103 pressing: Pressing by grinding or cold isostatic pressing, with a pressure of 150-200 MPa, into small balls or small cubes with a diameter of 20-50 mm.

[0110] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1500°C for 2-4 hours to obtain a rod.

[0111] S105 crushing: The rod is crushed to obtain tungsten-nickel-iron powder with a D50 of 33 microns.

[0112] S106 adopts SLM powder spreading 3D printing: same as Example 1.

[0113] Test Case

[0114] The tungsten-nickel-iron powder in step S105 of Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 1 and Figure 2 As shown. Figure 1 It can be seen that the surface of the spherical tungsten powder is relatively smooth, the shape is relatively regular, and the particle size is relatively uniform, basically around 32 microns.

[0115] from Figure 2 It can be seen more clearly that the surface of the spherical tungsten powder is relatively smooth and spherical, basically around 32 microns.

[0116] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a tungsten-nickel-iron component, characterized in that: include: Spreading tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component, printing, and obtaining a green body of the tungsten-nickel-iron component; The tungsten-nickel-iron powder is a solid structure with a particle size of 20-40 microns; the tungsten-nickel-iron powder includes tungsten particles and a metal layer covering the tungsten particles, and the metal layer is a nickel and iron metal layer; The green body of the tungsten-nickel-iron component is kept at 1100-1200° C. under vacuum for 3-10 hours, and cooled to obtain a tungsten-nickel-iron component; The preparation method of the tungsten-nickel-iron powder comprises: Mix tungsten powder, nickel powder and iron powder and grind them to obtain mixed powder; wherein the particle size of the tungsten powder is 20-40 microns, the particle size of the nickel powder is 1-3 microns, and the particle size of the iron powder is 1-3 microns; Granulating and pressing the mixed powder to obtain a material body; After degreasing the material blank at 800° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod; The rod is crushed, and particles with a crushed particle size of 25-53 microns are screened to obtain the tungsten-nickel-iron powder.

2. The preparation method according to claim 1, characterized in that: In the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing: The oxygen content in the molding chamber is less than 100ppm and the pressure is maintained at 10-40mbar; the laser power for scanning the entity is 400W, the laser power for scanning the contour is 200W, the laser power for supporting is 300W, the spot diameter is 50pm, the entity scanning speed is 1500mm / s, the contour scanning speed is 300mm / s, the support scanning speed is 2000mm / s, the scanning overlap rate is 0.06, and the substrate preheating temperature is 700℃.

3. The preparation method according to claim 2, characterized in that: In the step of spreading the tungsten-nickel-iron powder according to the designed shape of the tungsten-nickel-iron component and printing: A laser beam is used to quickly melt the powder according to the slice shape and scanning path. The preset powder thickness is 30 μm, and the powder supply is set to 3 times the powder thickness. After printing is completed, the tungsten-nickel-iron component is placed in the molding chamber for 3 hours.

4. The preparation method according to claim 1, characterized in that: The green body of the tungsten-nickel-iron component is kept at 1100-1200° C. under vacuum for 3-10 hours, and the cooling step comprises: The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, and evacuated to a vacuum degree of less than 10 -3 Pa, maintain annealing temperature at 1200°C, holding time for 4-5h, and cool with the furnace.

5. The preparation method according to claim 1, characterized in that: In the step of mixing tungsten powder, nickel powder and iron powder for ball milling, the ball milling medium is ethanol, and 1-3% paraffin is added to the ethanol; the ball milling time is 24-48 hours, and the ball-to-material ratio of the ball milling is 4:1, and the material is the sum of the tungsten powder, the nickel powder and the iron powder.

6. The preparation method according to claim 1, characterized in that: The step of granulating the mixed powder comprises: spray drying and granulating the mixed powder at a gas temperature of 150-200°C.

7. The preparation method according to claim 6, characterized in that: The mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa. The material green body is a sphere with a diameter of 20-50 mm or a block with a width of 20-50 mm.

8. A tungsten-nickel-iron component obtained by the preparation method according to any one of claims 1 to 7.

9. The tungsten-nickel-iron component according to claim 8, characterized in that: The tungsten-nickel-iron component includes a fragment unit, and the fragment unit has a diameter of 200 mm and a height of 240 mm.