A kind of concrete and its preparation method and application
By preparing polycarboxylic acid water reducing agent with low acid ether ratio, the problem of poor water excretion and slump of concrete is solved, significantly improving the concrete's ease and water excretion rate, improving construction performance and engineering quality .
Patent Information
- Application Number
- CN202111564991.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-20
AI Technical Summary
When using high-water-reducing water-reducing agents, existing concrete is prone to problems of segregation and poor slump, which leads to construction difficulties and hidden dangers in engineering quality. Common improvement methods such as adding viscosity regulators and gas induction agents. The intensity has a great impact.
Using a polycarboxylic acid water reducing agent, it is prepared in the presence of a chain transfer agent through the reaction of an initiator and a reducing agent through the combination of a specific molar ratio of acrylic monomer and polyether monomer and the catalyst, and is prepared in the presence of a chain transfer agent, forming a low Polycarboxylic acid water reducing agent with acid ether ratio is used to improve concrete and water excretion.
Effectively improve the ease of concrete and water discharge rate, improve construction performance, especially in the case of high powder content or poor grade of machine sand, significantly improve the maintenance performance and construction adaptability of concrete.
Smart Images

Figure CN116283028B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to concrete and a preparation method and application thereof. Background Art
[0002] China's construction market has experienced rapid growth in recent years, resulting in huge consumption of high-quality sand and gravel. In addition to environmental protection requirements, some materials such as machine-made sand with poor grading or containing a large amount of stone powder and mud are used as concrete raw materials in large quantities. Concrete segregation and bleeding, poor slump retention ability and other problems often occur, which brings great difficulties to concrete practitioners in construction and may also cause hidden dangers to project quality.
[0003] The carboxylic acid water-reducing agent commonly used in the industry is still a high water-reducing type water-reducing agent. Generally, in this type of water-reducing agent molecules, the ratio of the number of carboxyl-containing small molecule segments to the number of polyether monomer molecules is relatively high. Concrete prepared with this type of water-reducing agent is prone to segregation, bleeding, and bottoming, and is highly sensitive to the water-reducing agent dosage. For today's poor land, the use of this type of water-reducing agent will cause a lot of trouble to the construction.
[0004] To solve this problem, the industry generally adopts the method of compounding some additives to improve the state of concrete, such as adding viscosity regulators, air entraining agents, etc., but this kind of approach has limited improvement, especially for air entraining agents. Excessive amount of air entraining agents may even have a significant impact on the strength of concrete. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a concrete, which comprises at least a polycarboxylate water-reducing agent represented by formula (I):
[0006]
[0007] Wherein, R1, R2, and R3 are the same or different and are independently selected from H, C 1-4 Alkyl, -(CH2) m COOH, -(CH2) p OH, for example, selected from H, C 1-3 Alkyl, such as selected from H, methyl, ethyl;
[0008] m is an integer selected from 0 to 3, such as 0, 1, 2 or 3;
[0009] p is an integer selected from 1 to 4, such as 1, 2, 3 or 4;
[0010] R4, R5, R6 are the same or different and are independently selected from H, C 1-3 Alkyl; for example, selected from H, methyl;
[0011] Y is -O- or absent;
[0012] The ratio of a / b is selected from a number between 1.5 and 3.5;
[0013] n is a number from 22 to 130.
[0014] According to an embodiment of the present invention, a / b may be an integer or a decimal, for example, it is selected from 1.5, 1.85, 2, 2.2, 2.5, 2.6, 3, 3.2, 3.5, preferably an integer or a decimal selected from 1.7 to 3.2.
[0015] According to an embodiment of the present invention, n may be an integer or a decimal, for example, selected from 22, 30, 40, 50, 55.5, 60, 70, 80, 90, 100, 110, 120, 130, preferably a number selected from 40-70.
[0016] According to an embodiment of the present invention, the raw materials for preparing the polycarboxylate water-reducing agent represented by formula (I) may include acrylic monomers and polyether monomers.
[0017] According to an embodiment of the present invention, the acrylic monomer can be selected from at least one of acrylic acid, maleic anhydride, itaconic acid, methacrylic acid, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, n-butyl acrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate; preferably acrylic acid.
[0018] According to an embodiment of the present invention, the polyether monomer may be selected from at least one of methyl allyl alcohol polyoxyethylene ether, isopentanol polyoxyethylene ether, allyl polyoxyethylene ether, and vinyl polyoxyethylene ether.
[0019] According to an embodiment of the present invention, the molar ratio of acrylic monomer to polyether monomer is (1.5-3.5):1, for example, 1.5:1, 1.8:1, 2:1, 2:2, 2.3:1, 2.5:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.5:1 or any value between any two ranges.
[0020] According to an embodiment of the present invention, a method for preparing a polycarboxylate water-reducing agent represented by formula (I) comprises: reacting a polyether monomer, an acrylic monomer, an initiator and a reducing agent to prepare the polycarboxylate water-reducing agent represented by formula (I).
[0021] According to an embodiment of the present invention, the preparation method is carried out in the presence of a chain transfer agent.
[0022] Preferably, the preparation method is carried out in the presence of a catalyst represented by formula (C);
[0023]
M x
[0024] Wherein, M is selected from metal ions, selected from Mg 2+ 、Al 3+ , Cu 2+ 、Ni 2+ , Fe 3+ , Fe 2+ 、Ti 2+ One or more of;
[0025] L is a ligand containing a functional group, selected from one or more of a carbonyl compound, a phosphine-containing compound, and a nitrogen-containing compound; the carbonyl compound may be formic acid, acetic acid, oxalic acid, ammonium oxalate, etc.; the phosphine-containing compound may be a phosphonic acid compound or a salt thereof, such as hydroxyethylidene diphosphonic acid, pentasodium aminotrimethylene phosphonate, etc.; the nitrogen-containing compound may be sodium ethylenediaminetetraacetate, an ammonium salt, etc.; the coordination number x:y is 1:3 to 1:5.
[0026] Preferably, the preparation method of the polycarboxylate water-reducing agent is carried out in the presence of water.
[0027] According to an embodiment of the present invention, the initiator is selected from at least one of water-soluble free radical initiators such as hydrogen peroxide, persulfate or azobisisobutylamidine; the amount of the initiator can be 0.7-1.8% of the mass of the polyether monomer.
[0028] According to an embodiment of the present invention, the reducing agent is selected from at least one of L-ascorbic acid, Rongalite, sodium hypophosphite, sodium disulfite, ammonium ferrous sulfate, etc.;
[0029] The concentration of the reducing agent is 1-2 wt %; the amount of the reducing agent can be 0.1-0.4% of the mass of the polyether monomer, preferably 0.2-0.3%.
[0030] According to an embodiment of the present invention, the chain transfer agent is selected from at least one of mercaptoethanol, thioglycolic acid, mercaptopropionic acid, sodium bisulfite, sodium hypophosphite, isopropanol, sodium methacrylic acid, sodium allyl sulfonate, etc. The amount of the chain transfer agent can be 0.1-2% of the mass of the polyether monomer.
[0031] According to an embodiment of the present invention, the method for preparing the catalyst represented by formula (C) comprises: reacting a salt containing the above-mentioned metal ions with a chemical substance containing a functional group to prepare the catalyst.
[0032] According to an embodiment of the present invention, in the catalyst preparation, the reaction can be carried out in a solvent of water.
[0033] According to an embodiment of the present invention, during the preparation of the catalyst, the reaction may be carried out under heating conditions, for example, the reaction temperature may be 30 to 80°C, such as 40 to 60°C.
[0034] According to an embodiment of the present invention, in the catalyst preparation, the reaction time may be 0.5 to 10 hours, such as 2 to 4 hours.
[0035] According to an embodiment of the present invention, in the preparation of the catalyst, the mass ratio of the metal ion to the compound containing the functional group can be 1:1 to 10, preferably 1:1 to 6, and more preferably 1:2.
[0036] According to an embodiment of the present invention, during the preparation of the catalyst, the pH value of the reaction system may be 2 to 6. Optionally, the reaction may be carried out in the presence of a pH adjuster to allow the reaction to proceed at a desired pH value.
[0037] According to an embodiment of the present invention, in the catalyst preparation, the salt containing the above metal ions is selected from at least one of titanium sulfate, ferrous sulfate, ferric sulfate, nickel sulfate, aluminum sulfate, copper sulfate and magnesium sulfate.
[0038] According to an embodiment of the present invention, in the preparation of the catalyst, the chemical substance containing the functionalized group is the above-mentioned ligand containing the functionalized group.
[0039] According to an exemplary embodiment of the present invention, the preparation method of the polycarboxylate water-reducing agent may include the following steps:
[0040] S1. adding a polyether monomer, water and the above catalyst to a reactor;
[0041] S2. The acrylic acid ester monomer and water are mixed to prepare a dropwise solution A;
[0042] S3. The reducing agent and water are mixed evenly to prepare a dropwise addition solution B;
[0043] S4. The chain transfer agent and water are mixed evenly to prepare a dropwise addition liquid C;
[0044] S5. adding a portion of the acrylic monomer, a portion of the reducing agent, and / or a portion of the chain transfer agent to the reactor of step (1);
[0045] The droplet B in step S4 and the droplet C in step S5 can be separately used as droplets, or prepared together as a mixed droplet;
[0046] S6. adding the initiator to the reactor in step S2;
[0047] S7. Control the droplet speed so that the droplet A, the droplet B, and the droplet C are synchronously added to the reactor in step S6. After the droplet addition is completed, the mixture is kept warm and matured; and then an alkaline compound is added to adjust the pH to obtain the water reducing agent.
[0048] According to an embodiment of the present invention, in step S1, the mass ratio of the polyether monomer to water is (1-1.5):1, for example, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1.
[0049] According to an embodiment of the present invention, in step S1, the polyether monomer is firstly mixed with water and then the catalyst is added and mixed evenly.
[0050] According to an embodiment of the present invention, in step S2, the mass concentration of the acrylic monomer is 30-60 wt%, for example, 30 wt%, 40 wt%, 50 wt% or 60 wt%.
[0051] According to an embodiment of the present invention, the molar ratio of acrylic monomer to polyether monomer is (1.5-3.5):1, for example, 1.5:1, 1.8:1, 2:1, 2.3:1, 2.5:1, 2.8:1, 3:1, 3.5:1 or any value between any two ranges.
[0052] According to an embodiment of the present invention, in step S5, the acrylic monomer may be an aqueous solution of the acrylic monomer; the reducing agent may be an aqueous solution of the reducing agent; and the chain transfer agent may be an aqueous solution of the chain transfer agent.
[0053] According to an embodiment of the present invention, in step S5, the portion of acrylic monomers is 0-50wt% of the total acrylic monomers, such as 0, 5wt%, 10wt%, 20wt%, 30wt%, 33wt%, 35wt%, 40wt%, 45wt%, 50wt% or any value in between any two ranges.
[0054] According to an embodiment of the present invention, in step S5, the portion of the reducing agent is 0-50wt% of the total reducing agent mass, such as 0, 5wt%, 10wt%, 20wt%, 30wt%, 33wt%, 35wt%, 40wt%, 45wt%, 50wt% or any value between any two ranges.
[0055] According to an embodiment of the present invention, in step S5, the portion of the chain transfer agent is 0-50wt% of the total chain transfer agent mass, such as 0, 5wt%, 10wt%, 20wt%, 30wt%, 33wt%, 35wt%, 40wt%, 45wt%, 50wt% or any value between any two ranges.
[0056] According to an embodiment of the present invention, in step S7, the insulation temperature is 15-34° C.; the aging time is 0 to 2 hours, preferably, the aging time is 1 hour.
[0057] According to an embodiment of the present invention, in step S7, the alkaline compound may be, for example, at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, and the like.
[0058] According to an embodiment of the present invention, in step S7, the adjusted pH value is 2 to 6, preferably 5.
[0059] According to an embodiment of the present invention, in step S7, the starting temperature of the dropping is less than 25°C.
[0060] According to an embodiment of the present invention, in step S7, the heating rate during the dropwise addition is ≤1°C / 30min.
[0061] According to an embodiment of the present invention, the dripping liquids are controlled to be dripped simultaneously and the dripping is completed synchronously, and the dripping time is 1 to 7 hours.
[0062] In the present invention, the conversion rate of the monomers (including the polyether monomers and the acrylic monomers) is >90%, preferably >95%.
[0063] According to an embodiment of the present invention, the concrete components include, by mass: 12-18 parts of cement, 0-4 parts of mineral powder, 0-5 parts of fly ash, 0-3 parts of stone powder, 0-3 parts of mud powder, 40-55 parts of gravel, 20-40 parts of river sand and / or machine-made sand, 5-8 parts of water, and 0.05-0.3 parts of polycarboxylate water reducer.
[0064] In the present application, illustratively, when the fly ash is 0, it means that the fly ash is not present in the concrete component. When the fly ash is present in the concrete component, its content is greater than 0. For example, the fly ash content can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5 or 5.0.
[0065] According to an embodiment of the present invention, the concrete components include, by mass: 15-18 parts of cement, 2-4 parts of mineral powder, 1-4 parts of fly ash, 40-50 parts of gravel, 20-35 parts of machine-made sand, 6-8 parts of water, and 0.06-0.2 parts of a polycarboxylate water-reducing agent represented by formula (I).
[0066] According to an embodiment of the present invention, the concrete components include, by mass: 12-18 parts of cement, 2-4 parts of mineral powder, 1-4 parts of fly ash, 1-3 parts of stone powder, 1-3 parts of mud powder, 40-50 parts of gravel, 20-35 parts of machine-made sand, 6-8 parts of water, and 0.06-0.2 parts of a polycarboxylate water reducer represented by formula (I).
[0067] According to an embodiment of the present invention, the weight average molecular weight of the polycarboxylate water-reducing agent is 20,000-50,000, preferably 21,000-48,000, for example, 20,000, 21,000, 24,000, 28,500, 38,000, 48,000 or 50,000.
[0068] According to an embodiment of the present invention, the number average molecular weight of the polycarboxylate water-reducing agent is 6000-30000, for example, 9000-30000, such as 6000, 6500, 9800, 11000, 13800, 15000, 24000, 27000, 30000.
[0069] According to an embodiment of the present invention, the peak molecular weight of the polycarboxylate water-reducing agent is 7000-50000, for example, 16000-40000, such as 7000, 7300, 9800, 11500, 13800, 16000, 17000, 21000, 25000, 37000, 38000, 40000.
[0070] The present invention also provides a method for preparing the concrete, which comprises: mixing cement, gravel, river sand and / or machine-made sand, water, a polycarboxylate water-reducing agent represented by formula (I), and optionally mineral powder, and / or fly ash, and / or stone powder, and / or mud powder to prepare concrete.
[0071] According to an embodiment of the present invention, the method comprises: mixing cement, gravel, river sand and / or machine-made sand, water, a polycarboxylate water-reducing agent represented by formula (I), mineral powder, fly ash, stone powder and mud powder to prepare concrete.
[0072] According to an embodiment of the present invention, the cement is Portland cement.
[0073] According to an embodiment of the present invention, the fly ash is low-calcium fly ash.
[0074] According to an embodiment of the present invention, the river sand and / or machine-made sand has a particle size of 0.15-1.18 mm and a fineness modulus of 2-1.5.
[0075] The present invention also provides the application of the above concrete, which can be used in highways, high-speed railways, bridges, tunnels, nuclear power plants, underground integrated pipe networks or civil engineering projects.
[0076] Beneficial effects of the present invention:
[0077] The inventors unexpectedly found that after adding the polycarboxylate water-reducing agent represented by formula (I) to concrete, the workability and water bleeding rate of the concrete can be effectively improved, and at the same time, when the concrete powder content is high, the retention performance of the concrete can be effectively improved. In addition, when the concrete uses machine-made sand, under the conditions of powder content, mud content or machine-made sand grading gap, the low acid-to-ether ratio water-reducing agent can effectively improve the state of the concrete, enhance the construction performance, and has good local adaptability.
[0078] Terminology Explanation and Description
[0079] The term "C 1-4 The term "alkyl" refers to straight-chain and branched alkyl groups having 1, 2, 3 or 4 carbon atoms. For example, methyl, ethyl, propyl, butyl, isopropyl, isobutyl, sec-butyl, tert-butyl, etc. or isomers thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] Figure 1 This is the H NMR spectrum of the catalyst in Preparation Example 1.
[0081] Figure 2 This is the gel chromatogram of the water reducing agent in Preparation Example 1.
[0082] Figure 3 This is the H NMR spectrum of the water reducing agent in Preparation Example 1.
[0083] Figure 4 This is the H NMR spectrum of the catalyst in Preparation Example 3.
[0084] Figure 5 This is the H NMR spectrum of the catalyst in Preparation Example 5. DETAILED DESCRIPTION
[0085] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0086] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0087] Preparation of polycarboxylate water reducer
[0088] Preparation Example 1
[0089] 45g of methyl allyl alcohol polyoxyethylene ether (HPEG) with an Mn of 2400, 30g of water and 0.5g of catalyst were put into a reactor and stirred to dissolve and mix evenly; 3.05g of acrylic acid and 5g of water were prepared as droplet A, 0.1g of L-ascorbic acid, 0.4g of mercaptopropionic acid and 10g of water were prepared as droplet B; 1 / 3 of A and B were put into the bottom of the reactor and homogenized, and then 0.6g of hydrogen peroxide was added to the reactor, the initial reaction temperature T=20°C, ΔT=1°C / 30min, the remaining droplets A and B were added dropwise at a uniform speed, the addition was completed in 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and a water reducer sample (the acid-ether ratio of the water reducer a / b≈2.2) was obtained, and the prepared water reducer was recorded as s1.
[0090] The GPC (gel chromatography) spectrum of sample s1 is as follows Figure 2 shown.
[0091] The NMR spectrum of the water reducer is as follows Figure 3 shown. Figure 3 The integral of a (1.0-2.0 ppm) is 70, which is the integral area of polyacrylic acid, and the integral of b (3.5-4.1 ppm) is 1100, which is the integral area of polyether 2400. The calculation formula is (70 / 72): (1100 / 2400) = 2.2:1. The corresponding sample analysis indicators are shown in Table 1 below.
[0092] Table 1
[0093]
[0094]
[0095] Wherein, the preparation method of the catalyst is as follows:
[0096] 1g of nickel sulfate, 2g of ferrous sulfate, 2g of ethylenediaminetetraacetic acid disodium (EDTA-2Na) and 4g of hydroxyethylidene diphosphonic acid (HEDP) were dissolved in 90g of water. The pH value of the reaction system was 2-6. After reacting at 40°C for 2h, a stable complex aqueous solution was prepared to obtain a catalyst with the following structure. The hydrogen nuclear magnetic spectrum of the catalyst is as follows: Figure 1 As shown:
[0097]
[0098] Preparation Example 2
[0099] 45g of methyl allyl alcohol polyoxyethylene ether with Mn of 2400, 30g of water and 0.5g of the catalyst in Preparation Example 1 were put into a reactor and stirred to dissolve and mix evenly; 2.5g of acrylic acid and 5g of water were prepared as droplet A, 0.1g of L-ascorbic acid, 0.4g of mercaptopropionic acid and 10g of water were prepared as droplet B; 1 / 3 of A and B were put into the bottom of the reactor and homogenized, and then 0.6g of hydrogen peroxide was added to the reactor, the initial reaction temperature was controlled to be T = 20°C, ΔT = 1°C / 30min, and the remaining droplets A and B were uniformly added dropwise for 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the desired water reducer sample (the acid-ether ratio of the water reducer was about a / b≈2.2) was obtained, and the prepared water reducer was recorded as s2. The analytical indicators of sample s2 are shown in Table 2 below.
[0100] Table 2
[0101] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 24000 11000 21000 95.9
[0102] Preparation Example 3
[0103] 45g of methyl allyl alcohol polyoxyethylene ether with Mn of 2400, 30g of water and 0.5g of catalyst were added to the reactor and stirred to dissolve and mix evenly; 3g of acrylic acid, 1g of hydroxypropyl acrylate and 5g of water were used to prepare droplet A, 0.1g of L-ascorbic acid, 0.4g of mercaptopropionic acid and 10g of water were used to prepare droplet B; 1 / 3 of A and B were added to the bottom of the reactor and homogenized, and then 0.6g of hydrogen peroxide was added to the reactor, the initial reaction temperature was controlled to be T = 20°C, ΔT = 1°C / 30min, and the remaining droplets A and B were added dropwise at a uniform speed for 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the desired water reducer sample (the acid-ether ratio of the water reducer a / b≈2.6) was obtained, and the prepared water reducer was recorded as s3. The corresponding sample analysis indicators are shown in Table 3 below.
[0104] Table 3
[0105] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 21000 9800 17000 96.7
[0106] Wherein, the preparation method of the catalyst is as follows:
[0107] 1g titanium sulfate, 2g ferrous sulfate, 2g ethylenediaminetetraacetic acid disodium (EDTA-2Na), 4g hydroxyethylidene diphosphonic acid (HEDP) were dissolved in 90g water, the pH value of the reaction system was 2-6, and after reacting at 40°C for 2h, a stable complex aqueous solution was prepared, i.e., the catalyst shown in the following formula. The NMR hydrogen spectrum of the catalyst is as follows Figure 4 shown.
[0108]
[0109] Preparation Example 4
[0110] 45g of prenol polyoxyethylene ether (TPEG) with Mn of 2400, 30g of water and 0.5g of the catalyst in Preparation Example 3 were put into a reactor and stirred to dissolve and mix evenly; 3g of acrylic acid, 1g of n-butyl acrylate and 5g of water were prepared as droplet A, 0.15g of Rongalite and 5g of water were prepared as droplet B, and 0.4g of thioglycolic acid and 5g of water were prepared as droplet C; then 0.3g of hydrogen peroxide and 0.4g of ammonium persulfate were added to the reactor, the initial reaction temperature T = 20°C, ΔT = 1°C / 30min, and the droplet A, droplet B and droplet C were uniformly added dropwise for 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the desired water reducer sample (the acid-ether ratio of the water reducer a / b≈2.6) was obtained, and the prepared water reducer was recorded as s4. The corresponding sample analysis indicators are shown in Table 4 below.
[0111] Table 4
[0112] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 38000 15000 38000 97.7
[0113] Preparation Example 5
[0114] 45g of vinyl polyoxyethylene ether (VPEG) with Mn of 3000, 30g of water and 0.5g of catalyst were put into a reactor and stirred to dissolve and mix evenly; 3.5g of acrylic acid and 3.2g of water were used to prepare droplet A, 0.1g of L-ascorbic acid, 0.7g of sodium hypophosphite and 10g of water were used to prepare droplet B; 1 / 3 of A and B were put into the bottom of the reactor and homogenized, and then 0.8g of hydrogen peroxide was added to the reactor, the initial reaction temperature was controlled to be T=20°C, ΔT=1°C / 30min, and the remaining droplets A and B were added dropwise at a uniform speed for 1h, and the reaction was terminated by keeping warm for 0.5h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the desired water reducer sample (the acid-ether ratio of the water reducer a / b≈3.2) was obtained, and the prepared water reducer was recorded as s5. The corresponding sample analysis indicators are shown in Table 5 below.
[0115] Table 5
[0116] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 48000 27000 37000 98.4
[0117] Wherein, the preparation method of the catalyst is as follows:
[0118] 1g aluminum sulfate, 2g copper sulfate, 2g ammonium oxalate, and 4g aminotrimethylenephosphonic acid pentasodium were dissolved in 90g water, and the pH value of the reaction system was 2-6. After reacting at 50°C for 2h, a stable complex aqueous solution was prepared, i.e., a catalyst shown in the following structure. The NMR hydrogen spectrum of the catalyst is as follows Figure 5 shown.
[0119]
[0120] The deuterated reagent used in the nuclear magnetic resonance tests of the catalysts in Preparation Examples 1, 3, and 5 was deuterated water (produced by Qingdao Tenglong Microwave Technology Co., Ltd.).
[0121] Comparative Preparation Example 1
[0122] The water reducer s6 of comparative preparation example 1 is a commercially available water reducer (Jiangsu Chaoli Building Materials Technology Co., Ltd., brand C7 water-reducing mother liquor, wherein the acid-ether ratio water reducer: acid-ether ratio ≈ 4.7, the polyether monomer used is methyl allyl polyoxyethylene ether, and the polyether molecular weight is 3000). The water reducer information is shown in Table 6 below.
[0123] Table 6
[0124] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 46000 24000 45000 92.4
[0125] Comparative Preparation Example 2
[0126] The water reducer s7 of comparative preparation example 2 is a commercially available water reducer (Jiangsu Chaoli Building Materials Technology Co., Ltd., brand C3 water-reducing mother liquor, wherein the acid-ether ratio water reducer: acid-ether ratio ≈ 4.1, the polyether monomer used is methyl allyl polyoxyethylene ether, and the polyether molecular weight is 3000). The water reducer information is shown in Table 7 below.
[0127] Table 7
[0128] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 42000 26000 40000 84.6
[0129] Comparative Preparation Example 3
[0130] 45g of methyl allyl alcohol polyoxyethylene ether with Mn of 2400, 30g of water and 0.5g of the catalyst in Preparation Example 1 were put into a reactor and stirred to dissolve and mix evenly; 3.5g of acrylic acid and 5g of water were prepared as droplet A, 0.1g of L-ascorbic acid, 0.65g of mercaptopropionic acid and 10g of water were prepared as droplet B; 1 / 3 of A and B were put into the bottom of the reactor and homogenized, and then 0.6g of hydrogen peroxide was added to the reactor, the initial reaction temperature was controlled to be T = 20°C, ΔT = 1°C / 30min, and the remaining droplets A and B were uniformly added dropwise for 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the desired water reducer sample (the acid-ether ratio of the water reducer was about a / b≈2.6) was obtained, and the prepared water reducer was recorded as s8. The corresponding sample analysis indicators are shown in Table 8 below.
[0131] Table 8
[0132] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 10000 6500 9800 94.9
[0133] Comparative Preparation Example 4
[0134] 45g of methyl allyl alcohol polyoxyethylene ether with Mn of 2400 and 30g of water were added to the reactor, stirred, dissolved and mixed evenly; 3.5g of acrylic acid and 5g of water were prepared as drop solution A, 0.1g of L-ascorbic acid, 0.4g of mercaptopropionic acid and 10g of water were prepared as drop solution B; 1 / 3 of A and B were added to the bottom of the reactor and homogenized, and then 0.6g of hydrogen peroxide was added to the reactor, the initial reaction temperature was controlled to be T = 20°C, ΔT = 1°C / 30min, and the reaction was added dropwise at a uniform speed for 2h, and the reaction was terminated by keeping warm for 1h; after the reaction was completed, 30wt% of NaOH aqueous solution was added to adjust the pH to 5, and the water reducer s9 (the acid-ether ratio of the water reducer was about a / b≈2.6) was obtained. The corresponding sample analysis indicators are shown in Table 9.
[0135] Table 9
[0136] Weight average molecular weight Mw Number average molecular weight Mn Peak molecular weight Mp Monomer conversion rate % 32500 16500 31000 81.3
[0137] The parameters of each water reducing agent in Preparation Examples 1-5 and Comparative Preparation Examples 1-4 are shown in Table 10:
[0138] Table 10
[0139]
[0140] Concrete preparation
[0141] Examples 1 to 5 and Comparative Examples 1 to 4
[0142] The water reducing agents prepared in Preparation Examples 1 to 5 and Comparative Preparation Examples 1 to 4 were added to the concrete mixed with clean machine-made sand. The concrete proportions used were shown in Table 11, and the prepared concretes were respectively recorded as Examples 1 to 5 and Comparative Examples 1 to 4.
[0143] Table 11
[0144] Southern 42.5 cement Fly ash Mineral powder Machine-made sand Stone water Polycarboxylate water reducer 17.3 servings 1.7 servings 2.7 servings 25.8 copies 45.8 copies 6.6 servings 0.1 part
[0145] The test data of the concrete prepared in Examples 1 to 5 and Comparative Examples 1 to 4 are shown in Table 12:
[0146] For the test methods of the parameters in Table 12, please refer to the national standard GB / T50081-2016.
[0147] Table 12
[0148]
[0149]
[0150] Note: ★ indicates 1 star, ☆ indicates 0.5 star, and workability is a comprehensive index obtained from surface observation, which reflects the uniformity of the concrete state, the workability, etc. The better the workability, the more stars it will get.
[0151] The above data show that when the concrete contains a water reducer with a low acid-ether ratio, a weight average molecular weight between 20,000-50,000, and a conversion rate greater than 95%, the workability of the resulting mixed machine-made sand concrete and the subsequent strength properties are very good.
[0152] Examples 6 to 10 and Comparative Examples 5 to 8
[0153] The water reducing agents prepared in Preparation Examples 1 to 5 and Comparative Preparation Examples 1 to 4 were added to concrete mixed with machine-made sand and stone powder and mud powder. The concrete proportions were shown in Table 13, and the prepared concretes were respectively recorded as Examples 6 to 10 and Comparative Examples 5 to 8.
[0154] Table 13
[0155]
[0156] The test data of the concrete prepared in Examples 6 to 10 and Comparative Examples 5 to 8 are shown in Table 14:
[0157] Table 14
[0158]
[0159]
[0160] Note: ★ indicates 1 star, ☆ indicates 0.5 star, and workability is a comprehensive index obtained from surface observation, which reflects the uniformity of the concrete state, the workability, etc. The better the workability, the more stars it will get.
[0161] The data in Table 6 show that when the concrete contains a water-reducing agent with a low acid-ether ratio, a weight-average molecular weight between 20,000 and 50,000, and a conversion rate greater than 95%, even if part of the machine-made sand in the concrete is replaced by the same amount of mud powder and stone powder, the resulting concrete has better retention capacity than the water-reducing agent with a relatively high acid-ether ratio, and it also has good test results in workability and later strength.
[0162] According to the above test results, as environmental protection policies become increasingly stringent, natural high-quality sand and gravel are consumed in large quantities and some inferior ones have to be widely used as concrete materials. The low acid-to-ether ratio water reducer prepared by the present application can effectively improve the state of concrete and provide an effective method to solve the problem for the convenience of engineering construction and the improvement of engineering quality.
[0163] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A concrete, characterized in that: The concrete at least comprises a polycarboxylate water-reducing agent represented by formula (I): (I); Wherein, R1, R2, and R3 are the same or different and are independently selected from H, C 1-4 Alkyl, -(CH2) m COOH, -(CH2) p OH; m is an integer selected from 0 to 3; p is an integer selected from 1 to 4; R4, R5, R6 are the same or different and are independently selected from H, C 1-3 alkyl; Y is -O- or absent; The ratio of a / b is selected from a number between 1.5 and 3.2; n is a number between 22 and 130; The preparation method of the polycarboxylate water reducer represented by formula (I) comprises: reacting a polyether monomer, an acrylic monomer, an initiator and a reducing agent to prepare the polycarboxylate water reducer represented by formula (I); The method for preparing the polycarboxylate water-reducing agent represented by formula (I) is carried out in the presence of a catalyst represented by formula (C); 【M x 】L y (C) Wherein, M is selected from metal ions, selected from Mg 2+ 、Al 3+ , Cu 2+ 、Ni 2+ , Fe 3+ , Fe 2+ 、Ti 2+ One or more of; L is a ligand containing a functional group, selected from one or more of a carbonyl compound, a phosphine-containing compound, and a nitrogen-containing compound; the carbonyl compound is formic acid, acetic acid, oxalic acid, or ammonium oxalate; the phosphine-containing compound is hydroxyethylidene diphosphonic acid or pentasodium aminotrimethylene phosphonate; the nitrogen-containing compound is sodium ethylenediaminetetraacetate or an ammonium salt; the coordination number x:y is 1:3 to 1:5; The weight average molecular weight of the polycarboxylate water reducer is 20,000-50,000.
2. The concrete according to claim 1, characterized in that The method for preparing the polycarboxylate water-reducing agent represented by formula (I) is carried out in the presence of a chain transfer agent.
3. The concrete according to claim 1, characterized in that The preparation method of the catalyst represented by formula (C) comprises: reacting a salt containing the above-mentioned metal ions with a chemical substance containing a functional group to prepare the catalyst.
4. The concrete according to claim 3, characterized in that The salt containing the above metal ions is selected from at least one of titanium sulfate, ferrous sulfate, ferric sulfate, nickel sulfate, aluminum sulfate, copper sulfate, and magnesium sulfate; The chemical substance containing a functional group is the ligand containing a functional group.
5. The concrete according to claim 1, characterized in that The concrete components include, by weight: 12-18 parts of cement, 0-4 parts of mineral powder, 0-5 parts of fly ash, 0-3 parts of stone powder, 0-3 parts of mud powder, 40-55 parts of gravel, 20-40 parts of river sand and / or machine-made sand, 5-8 parts of water, and 0.05-0.3 parts of a polycarboxylate water reducer represented by formula (I).
6. The concrete according to claim 5, characterized in that The concrete components include, by weight: 15-18 parts of cement, 2-4 parts of mineral powder, 1-4 parts of fly ash, 40-50 parts of gravel, 20-35 parts of machine-made sand, 6-8 parts of water, and 0.06-0.2 parts of a polycarboxylate water reducer represented by formula (I).
7. The concrete according to claim 5, characterized in that The concrete components include, by weight: 12-18 parts of cement, 2-4 parts of mineral powder, 1-4 parts of fly ash, 1-3 parts of stone powder, 1-3 parts of mud powder, 40-50 parts of gravel, 20-35 parts of machine-made sand, 6-8 parts of water, and 0.06-0.2 parts of a polycarboxylate water reducer represented by formula (I).
8. The concrete according to claim 1, characterized in that The weight average molecular weight of the polycarboxylate water reducer is 21000-48000; The number average molecular weight of the polycarboxylate water reducer is 6000-30000; The peak molecular weight of the polycarboxylate water-reducing agent is 7000-50000.
9. The method for preparing concrete according to claim 5, characterized in that: The concrete components are mixed in parts by mass to prepare concrete.
10. The preparation method according to claim 9, characterized in that: The method comprises: mixing cement, gravel, river sand and / or machine-made sand, water, a polycarboxylate water-reducing agent represented by formula (I), mineral powder, fly ash, stone powder and mud powder to prepare concrete.
11. Use of the concrete according to any one of claims 1 to 8 in highways, high-speed railways, bridges, tunnels, nuclear power plants, underground integrated pipe networks or civil engineering projects.