A low stress bonding adhesive material and preparation method
By introducing cyclopentadiene into cyclic olefin copolymer resin to form polycyclopentadiene, the problem of balancing temperature resistance and stress in existing temporary bonding adhesive materials is solved, achieving improved strength and toughness at high temperatures while maintaining washability.
Patent Information
- Application Number
- CN202310130442.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-17
AI Technical Summary
Existing temporary bonding adhesive materials cannot simultaneously achieve high temperature resistance and low stress, resulting in wafers being prone to breakage and deformation during the thinning process.
By introducing cyclopentadiene into cyclic olefin copolymer resins to form polycyclopentadiene, toughness and cross-linking structure are improved, high-temperature bonding strength is enhanced, and stress is reduced.
The prepared low-stress bonding adhesive material has good bonding strength and low residual stress at high temperatures, which can effectively prevent wafer breakage and deformation, and can be cleaned in specific solvents.
Smart Images

Figure CN116285709B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a bonding adhesive material and a preparation method thereof. Background Art
[0002] The end of device scaling based on Moore's Law and the next generation of lithography that will continue this legendary law have been the subject of debate for nearly a decade. Faced with increasing challenges, three-dimensional (3D) devices have become a viable solution for making smaller, faster, and more powerful devices. Three-dimensional integration and packaging require new methods to process and handle wafers. Typically, 3D structures made by through-silicon vias (TSVs) are considered 3D integration. Most stacked devices, which usually involve wafer thinning processes and require some thin wafer handling methods, have proven to be handled without significant damage to wafers thinned to 150μm or thinner, but these wafers require highly complex and expensive equipment to handle to avoid damage. When the thickness is greater than 100μm, the formation and filling of TSVs will be difficult and expensive. With thinner substrates, interconnect delays and heat dissipation issues can be better addressed. For TSV technology to be feasible, wafers must be thinned to 100μm or thinner. Thinned silicon wafers are very fragile and often have distortions and dents, and this risk increases with the increase in wafer size. Most 3D integrated circuit (IC) manufacturers are eager to reduce wafer thickness to 50μm or less to realize the full benefits of 3D integration. Handling such thin wafers requires that each wafer be temporarily bonded to a carrier or handle wafer using a temporary bonding material. Once a device wafer is attached to a carrier wafer, the wafer pair can be handled like a standard full-thickness wafer. When backside processing is completed, the thinned wafer can be separated (released or peeled) from the carrier and attached to a dicing frame to be singulated into chips for the pick-up process.
[0003] During use, temporary bonding adhesive materials usually need to withstand the high shear force caused by the thinning process, while ensuring that the device wafer is fixed on the carrier without sliding or tilting. In addition, temporary bonding adhesives also need to undergo various processing processes together with the device wafer, such as high temperature (250°C or higher), chemical reagent treatment (polar solvents, strong acids), etc. At present, the mainstream temporary bonding adhesive materials are mainly made of thermoplastic resins as the main raw materials, and the most widely used is cycloolefin copolymer. Cycloolefin copolymer resins have good high temperature resistance, medium resistance, high transparency and other characteristics, but cycloolefin copolymer resins also have the problem of greater brittleness, which also leads to stress concentration during the thinning process when used as temporary bonding adhesive materials, resulting in wafer fragmentation, and it is also easy to accumulate thermal stress when experiencing large temperature changes, causing deformation of the device wafer. Moreover, due to the poor compatibility of cycloolefin copolymer resins with conventional thermoplastic elastomers, the industry often increases the flexibility of temporary bonding adhesive materials by selecting cycloolefin copolymer resins with lower molecular weights, but this also greatly reduces the heat resistance of the material. Therefore, it is necessary to develop a toughening resin that has good compatibility with the cycloolefin copolymer resin, and to obtain a temporary bonding adhesive material that has both heat resistance and low stress properties by blending with the cycloolefin copolymer resin. Summary of the invention
[0004] The present invention aims to solve the problem that existing temporary bonding adhesive materials cannot achieve both high temperature resistance and low stress, and further provide a low stress bonding adhesive material and a preparation method thereof.
[0005] A low stress bonding adhesive material is prepared by 100 parts by mass of a cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant, and 100 to 250 parts of a solvent;
[0006] The cyclopentadiene is dicyclopentadiene or 1-pentyl-2,4-cyclopentadiene;
[0007] The structural formula of the dicyclopentadiene is
[0008] The structural formula of the 1-pentyl-2,4-cyclopentadiene is
[0009] A method for preparing a low stress bonding adhesive material is carried out according to the following steps:
[0010] 1. Weigh 100 parts of cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant, and 100 to 250 parts of a solvent by mass;
[0011] 2. Add the weighed cycloolefin copolymer resin to the solvent, stir for 4h to 6h under a nitrogen atmosphere and a temperature of 50℃ to 120℃, then stop heating and continue stirring. After cooling to room temperature, add an antioxidant. After the antioxidant is dissolved, add the cyclopentadiene premixed with the catalyst at a feeding time of 30min to 90min, and continue stirring at room temperature for 1h to 4h to obtain a low stress bonding adhesive material.
[0012] The beneficial effects of the present invention are:
[0013] Cyclopentadiene is introduced into cycloolefin copolymer resin, and after heat treatment, cyclopentadiene can be cross-linked and polymerized into polycyclopentadiene. Polycyclopentadiene has excellent toughness, effectively makes up for the larger shortcoming of cycloolefin copolymer resin brittleness, and this makes the temporary bonding adhesive material prepared by the present invention possess the characteristic of low stress. In addition, polycyclopentadiene makes the whole system in a three-dimensional cross-linked structure, effectively improves the high-temperature modulus of material, and further strengthens high-temperature bonding strength.
[0014] The present invention adopts cycloolefin copolymer resin as the main component of the temporary bonding adhesive material and cyclopentadiene as the modifier. Compared with the temporary bonding adhesive material of the pure cycloolefin copolymer resin system, the bonding strength at high temperature is improved and the stress of the material during use is reduced. In addition, the cycloolefin copolymer resin unexpectedly has good compatibility with cyclopentadiene in a specific solvent. The above three properties are satisfied at the same time, which is difficult to achieve with other types of modifiers (such as low molecular weight cycloolefin copolymers, polycarbonate, polystyrene, rubber, epoxy resin).
[0015] Compared with conventional cyclopentadiene, the 1-pentyl-2,4-cyclopentadiene synthesized by the present invention has an additional pentyl structure, and after polymerization, the flexibility of the molecular chain segment is improved. At the same time, the pentyl on its side chain increases the irregularity of the molecular structure to a certain extent, resulting in a decrease in its cross-linking density, so that the thermoplastic cycloolefin molecules can be better distributed in its skeleton structure, which not only has a better toughening effect, but also brings lower residual stress to the cycloolefin copolymer system, and also ensures the washability of the prepared bonding adhesive material.
[0016] The present invention uses a residual stress tester to effectively evaluate the stress generated by the temporary bonding adhesive material under various temperature environments, and intuitively quantifies the magnitude of the stress.
[0017] The temporary bonding adhesive material prepared by the present invention has the following advantages:
[0018] (1) It has high thermal stability, and no defects are generated at 350℃ / 120min after bonding;
[0019] (2) Good bonding performance, high chip shear strength at room temperature and high temperature, the room temperature shear strength is ≥14MPa, and the shear strength at 150℃ is ≥5MPa;
[0020] (3) It has low stress characteristics and can produce lower residual stress after high temperature treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the infrared spectrum of 1-pentyl-2,4-cyclopentadiene prepared in Example 5. DETAILED DESCRIPTION
[0022] Specific implementation method 1: A low stress bonding adhesive material of this implementation method is prepared by 100 parts of cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant and 100 to 250 parts of a solvent in parts by mass;
[0023] The cyclopentadiene is dicyclopentadiene or 1-pentyl-2,4-cyclopentadiene;
[0024] The structural formula of the dicyclopentadiene is
[0025] The structural formula of the 1-pentyl-2,4-cyclopentadiene is
[0026] The cycloolefin copolymer resin in this embodiment is usually selected from a weight average molecular weight (M w ) in the range of 50,000 to 300,000, preferably 80,000 to 250,000, more preferably 100,000 to 200,000. The cycloolefin copolymer resin also preferably has a glass transition temperature (Tg) of 80°C or higher, more preferably 90°C to 170°C. Typical cycloolefin copolymer resins used in this embodiment can be Polyplastics Co., Ltd. Series products, Japan JSR company Series of products, etc.
[0027] In this specific embodiment, the amount of cyclopentadiene premixed with the catalyst is generally 2 to 10 parts, preferably 2 to 8 parts, and more preferably 3 to 5 parts, relative to 100 parts by mass of the cycloolefin copolymer resin. Too much cyclopentadiene will cause the entire system to have too high a crosslinking density after heating, and it will not be possible to clean it with a specific solvent, while too low a cyclopentadiene ratio will make it difficult for the system to crosslink, and it will not have a toughening effect.
[0028] The catalyst used in this embodiment is a compound that enables cyclopentadiene to undergo a cross-linking reaction at a certain temperature.
[0029] The antioxidant used in this embodiment is preferably 0.1 to 0.2 parts by mass.
[0030] In this embodiment, the amount of the solvent used is generally 100 to 250 parts, preferably 100 to 200 parts, and more preferably 150 to 200 parts, relative to 100 parts by mass of the cycloolefin copolymer resin. The solvent system should have a boiling point of about 100°C to 230°C, preferably 120°C to 200°C, and more preferably 140°C to 190°C.
[0031] The temporary bonding adhesive material of this specific embodiment is an adhesive material with heat resistance and low stress characteristics, which can be used to fix the device wafer on the carrier and can be cleaned by a specific solution after separation.
[0032] The temporary bonding adhesive material of this specific embodiment can withstand a long-term high temperature environment (350°C or higher), and compared with conventional temporary bonding adhesive materials, the temporary bonding adhesive material of this specific embodiment generates less stress when experiencing temperature changes, and is less likely to cause warping or debonding, thereby reducing the possibility of device wafer damage. Compared with other low-stress temporary bonding adhesive materials, the temporary bonding adhesive material of this specific embodiment has better heat resistance.
[0033] The purpose of this specific embodiment is that cycloolefin copolymer resin is difficult to be well miscible with conventional elastomers in a solvent, and by introducing a certain amount of cyclopentadiene into the cycloolefin copolymer resin, good miscibility can be achieved in the solvent. At the same time, during the heating and bonding process, cyclopentadiene can be cross-linked and polymerized to a certain extent into polycyclopentadiene under the action of a catalyst, which has a good toughening effect on the cycloolefin copolymer resin. When used as a temporary bonding adhesive material, it not only improves the bonding strength, but also unexpectedly reduces the stress of the material during use. Through residual stress testing, the stress value at high temperature has been effectively reduced.
[0034] Another purpose of this specific embodiment is that the cross-linked polycyclopentadiene has a higher modulus and has more cyclic structures in the molecular structure, so that it can maintain a certain strength at high temperatures, which effectively improves the high temperature performance of the cycloolefin copolymer resin, thereby making up for the shortcoming of insufficient heat resistance of the temporary bonding adhesive material. In addition, by controlling the addition ratio of cyclopentadiene and the catalyst, the temporary bonding adhesive material can still be quickly and thoroughly cleaned by a specific solvent.
[0035] The beneficial effects of this specific implementation are:
[0036] Cyclopentadiene is introduced into cycloolefin copolymer resin, and after heat treatment, cyclopentadiene can be cross-linked and polymerized into polycyclopentadiene. Polycyclopentadiene has excellent toughness, effectively makes up for the larger shortcoming of cycloolefin copolymer resin brittleness, which makes the temporary bonding adhesive material prepared by this specific embodiment possess the characteristic of low stress. In addition, polycyclopentadiene makes the whole system in a three-dimensional cross-linked structure, effectively improves the high temperature modulus of the material, and further strengthens the high temperature bonding strength.
[0037] This specific embodiment uses cycloolefin copolymer resin as the main component of the temporary bonding adhesive material and cyclopentadiene as a modifier. Compared with the temporary bonding adhesive material of the pure cycloolefin copolymer resin system, the bonding strength at high temperature is improved and the stress of the material during use is reduced. In addition, the cycloolefin copolymer resin unexpectedly has good compatibility with cyclopentadiene in specific solvents. The above three properties are satisfied at the same time, which is difficult to achieve with other types of modifiers (such as low molecular weight cycloolefin copolymers, polycarbonate, polystyrene, rubber, epoxy resin).
[0038] Compared with conventional cyclopentadiene, the 1-pentyl-2,4-cyclopentadiene synthesized in this specific embodiment has an additional pentyl structure, which improves the flexibility of the molecular chain segments after polymerization. At the same time, the pentyl on its side chain increases the irregularity of the molecular structure to a certain extent, resulting in a decrease in its cross-linking density, so that the thermoplastic cycloolefin molecules can be better distributed in its skeleton structure, which not only has a better toughening effect, but also brings lower residual stress to the cycloolefin copolymer system, and also ensures the cleanability of the prepared bonding adhesive material.
[0039] This specific implementation uses a residual stress tester to effectively evaluate the stress generated by the temporary bonding adhesive material under various temperature environments, and intuitively quantifies the magnitude of the stress.
[0040] The temporary bonding adhesive material prepared by this specific implementation has the following advantages:
[0041] (1) It has high thermal stability, and no defects are generated at 350℃ / 120min after bonding;
[0042] (2) Good bonding performance, high chip shear strength at room temperature and high temperature, the room temperature shear strength ≥ 14MPa, the shear strength at 150℃ ≥ 5MPa;
[0043] (3) It has low stress characteristics and can produce lower residual stress after high temperature treatment.
[0044] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the weight average molecular weight of the cycloolefin copolymer resin is 50,000 to 300,000, and the glass transition temperature is above 80° C. Other aspects are the same as those of specific embodiment 1.
[0045] Specific embodiment 3: This embodiment is different from specific embodiment 1 or 2 in that the catalyst is one or a mixture of trinonylphenol tungsten trichloride, diethylaluminum monochloride, ethylaluminum dichloride, diisobutylaluminum chloride, methylaluminum dichloride and dimethylaluminum chloride. The rest is the same as specific embodiment 1 or 2.
[0046] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the antioxidant is a phenolic antioxidant or a phosphite antioxidant. The rest is the same as specific embodiments 1 to 3.
[0047] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the antioxidant is a mixture of one or both of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and tris(2,4-di-tert-butylphenyl)phosphite. Other aspects are the same as specific embodiments 1 to 4.
[0048] In this specific embodiment, the Cas of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) is 6683-19-8.
[0049] In this specific embodiment, the Cas of tris(2,4-di-tert-butylphenyl)phosphite is 31570-04-4.
[0050] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the boiling point of the solvent is 100° C. to 230° C. The rest is the same as specific implementation methods 1 to 5.
[0051] Specific embodiment 7: This embodiment is different from specific embodiments 1 to 6 in that the solvent is dipentene, 1-dodecene, cyclododecene, pinene, dicyclohexene, cyclooctane, cyclopentane, cycloheptane, butanone, cyclohexanone, cyclopentanone, D-limonene or butylcyclohexane. Others are the same as specific embodiments 1 to 6.
[0052] Specific embodiment eight: This embodiment differs from any one of specific embodiments one to seven in that: the 1-pentyl-2,4-cyclopentadiene is prepared according to the following steps:
[0053] ①Heat dicyclopentadiene to 140°C to 180°C, collect the fraction at 37°C to 42°C to obtain liquid cyclopentadiene, and seal and store the liquid cyclopentadiene at a low temperature of 0°C or below for future use;
[0054] ② Using tetrahydrofuran to dissolve liquid cyclopentadiene to obtain a tetrahydrofuran solution of cyclopentadiene; under nitrogen protection, adding tetrahydrofuran to NaH and dissolving it to obtain a reaction system, keeping the reaction system at 0°C under ice bath conditions, slowly dropping the tetrahydrofuran solution of cyclopentadiene into the reaction system at a dropping speed of 0.5mL / s to 1mL / s, reacting for 4h to 6h to obtain a purple-red solution of CPD-Na, and sealing and storing at low temperature for later use;
[0055] The mass ratio of NaH in the reaction system to cyclopentadiene in the tetrahydrofuran solution of cyclopentadiene is 1:(2-2.5);
[0056] ③ Under nitrogen atmosphere, add the tetrahydrofuran solution of 1-chloropentane dropwise into the purple-red solution of CPD-Na over 2 to 4 hours to obtain a solution of 1-pentyl-2,4-cyclopentadiene;
[0057] The molar ratio of CPD-Na in the purple-red solution of CPD-Na to 1-chloropentane in the tetrahydrofuran solution of 1-chloropentane is 1:(1-1.1);
[0058] ④ Extract the solvent from the 1-pentyl-2,4-cyclopentadiene solution by reducing pressure, then wash with water, extract and purify by rotary evaporation, and finally obtain a light yellow oily liquid, namely 1-pentyl-2,4-cyclopentadiene;
[0059] The mass percentage of the tetrahydrofuran solution of cyclopentadiene in step ② is 10% to 20%; the mass percentage of NaH in the reaction system in step ② is 5% to 15%; the mass percentage of the tetrahydrofuran solution of 1-chloropentane in step ③ is 8% to 15%. Others are the same as those in specific embodiments 1 to 7.
[0060] The liquid cyclopentadiene has a pungent odor and is colorless and transparent.
[0061] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the cyclopentadiene premixed with the catalyst is prepared according to the following steps: 100 parts of cyclopentadiene, 0.05 to 0.2 parts of catalyst and 240 to 400 parts of chloroform solution are weighed by mass, the weighed cyclopentadiene is added to the chloroform solution, and then the catalyst is added, stirred at room temperature for 1h to 4h, and the chloroform solution is removed by reduced pressure distillation to obtain the cyclopentadiene premixed with the catalyst. The rest is the same as specific embodiments 1 to 8.
[0062] Specific embodiment 10: This embodiment is a method for preparing a low stress bonding adhesive material, which is carried out according to the following steps:
[0063] 1. Weigh 100 parts of cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant, and 100 to 250 parts of a solvent by mass;
[0064] 2. Add the weighed cycloolefin copolymer resin to the solvent, stir for 4h to 6h under a nitrogen atmosphere and a temperature of 50℃ to 120℃, then stop heating and continue stirring. After cooling to room temperature, add an antioxidant. After the antioxidant is dissolved, add the cyclopentadiene premixed with the catalyst at a feeding time of 30min to 90min, and continue stirring at room temperature for 1h to 4h to obtain a low stress bonding adhesive material.
[0065] The following examples are used to verify the beneficial effects of the present invention:
[0066] Embodiment 1:
[0067] A method for preparing a low stress bonding adhesive material is carried out according to the following steps:
[0068] 1. Weigh 100 parts of cycloolefin copolymer resin, 2 parts of cyclopentadiene premixed with a catalyst, 0.2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 170 parts of 1-dodecene and 30 parts of cyclododecene by mass;
[0069] The cyclopentadiene premixed with the catalyst is specifically prepared according to the following steps: 100 parts of cyclopentadiene, 0.05 parts of trinonylphenol tungsten trichloride, 0.1 parts of diethylaluminum monochloride and 300 parts of chloroform solution are weighed by mass, the weighed cyclopentadiene is added to the chloroform solution, and then the catalyst is added, stirred at room temperature for 2 hours, and the chloroform solution is removed by reduced pressure distillation to obtain the cyclopentadiene premixed with the catalyst;
[0070] The cyclopentadiene is dicyclopentadiene;
[0071] The structural formula of the dicyclopentadiene is
[0072] The 100 parts of cycloolefin copolymer resin are specifically 70 parts of cycloolefin copolymer A1 ( F4520, commercially available) and 30 parts of cycloolefin copolymer A2 ( FBK80, commercially available); the weight average molecular weight of the cycloolefin copolymer A1 is 120,000, and the glass transition temperature is 146°C; the weight average molecular weight of the cycloolefin copolymer A2 is 160,000, and the glass transition temperature is 153°C;
[0073] 2. Add the weighed cycloolefin copolymer resin to 1-dodecene and cyclododecene, stir for 5 hours under a nitrogen atmosphere and a temperature of 80°C, then stop heating and continue stirring. After cooling to room temperature, add tri(2,4-di-tert-butylphenyl)phosphite. After the tri(2,4-di-tert-butylphenyl)phosphite is dissolved, add cyclopentadiene premixed with the catalyst at a feeding time of 30 to 45 minutes, and continue stirring at room temperature for 2 hours to obtain a low stress bonding adhesive material.
[0074] The dicyclopentadiene is a TCI reagent with 97% purity and is commercially available;
[0075] The diethylaluminum monochloride is TCI reagent, AR, commercially available;
[0076] The trinonylphenol tungsten trichloride is prepared according to the following steps:
[0077] Under nitrogen protection, nonylphenol and tungsten hexachloride in a molar ratio of 3:1 are dissolved in xylene, stirred at 65°C for 12 hours, and xylene is removed by reduced pressure distillation to obtain trinonylphenol tungsten trichloride; the mass ratio of nonylphenol to xylene is 1:5.
[0078] Example 2: This example is different from Example 1 in that: in step 1, 100 parts of cycloolefin copolymer resin, 3 parts of cyclopentadiene premixed with a catalyst, 0.2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 160 parts of 1-dodecene and 40 parts of cyclododecene are weighed by mass; in step 2, the cyclopentadiene premixed with the catalyst is added at a feeding time of 30 to 45 minutes, and stirring is continued at room temperature for 3 hours. The rest is the same as Example 1.
[0079] Embodiment 3: This embodiment is different from Embodiment 1 in that: in step 1, 100 parts of cycloolefin copolymer resin, 5 parts of cyclopentadiene premixed with the catalyst, 0.2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 160 parts of 1-dodecene and 40 parts of cyclododecene are weighed by mass; the cyclopentadiene premixed with the catalyst is prepared by the following steps: 100 parts of cyclopentadiene, 0.08 parts of trinonylphenol tungsten trichloride and 300 parts of chloroform solution are weighed by mass, the weighed cyclopentadiene is added to the chloroform solution, then the catalyst is added, stirred at room temperature for 2 hours, and the chloroform solution is removed by reduced pressure distillation to obtain the cyclopentadiene premixed with the catalyst; in step 2, the cyclopentadiene premixed with the catalyst is added at a feeding time of 45min to 60min, and stirring is continued at room temperature for 4h. The rest is the same as Embodiment 1.
[0080] Embodiment 4: This embodiment is different from Embodiment 1 in that: in step 1, 100 parts of cycloolefin copolymer resin, 8 parts of cyclopentadiene premixed with catalyst, 0.2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 150 parts of 1-dodecene and 50 parts of cyclododecene are weighed by mass; the cyclopentadiene premixed with catalyst is prepared by the following steps: 100 parts of cyclopentadiene, 0.05 parts of trinonylphenol tungsten trichloride and 300 parts of chloroform solution are weighed by mass, the weighed cyclopentadiene is added to the chloroform solution, then the catalyst is added, stirred at room temperature for 2 hours, and the chloroform solution is removed by reduced pressure distillation to obtain the cyclopentadiene premixed with catalyst; in step 2, the mixture is stirred for 6 hours under nitrogen atmosphere and temperature of 80°C; in step 2, the cyclopentadiene premixed with catalyst is added at a feeding time of 60min to 90min, and stirring is continued at room temperature for 6 hours. The rest is the same as in Embodiment 1.
[0081] Embodiment 5: This embodiment is different from Embodiment 1 in that: the cyclopentadiene described in step 1 is 1-pentyl-2,4-cyclopentadiene;
[0082] The structural formula of the 1-pentyl-2,4-cyclopentadiene is
[0083] The 1-pentyl-2,4-cyclopentadiene is specifically prepared according to the following steps:
[0084] ①Heat dicyclopentadiene to 160°C, collect the fraction at 37°C to 42°C to obtain liquid cyclopentadiene, and seal and store the liquid cyclopentadiene at a low temperature of 0°C or below for future use;
[0085] ② Use tetrahydrofuran to dissolve liquid cyclopentadiene to obtain a tetrahydrofuran solution of cyclopentadiene; under nitrogen protection, add tetrahydrofuran to NaH and dissolve it to obtain a reaction system, keep the reaction system at 0°C under ice bath conditions, slowly drop the tetrahydrofuran solution of cyclopentadiene into the reaction system at a drop rate of 1 mL / s, react for 5 hours, obtain a purple-red solution of CPD-Na, and seal and store at low temperature for later use;
[0086] The mass percentage of the tetrahydrofuran solution of cyclopentadiene is 10%; the mass percentage of NaH in the reaction system is 10%;
[0087] The mass ratio of NaH in the reaction system to cyclopentadiene in the tetrahydrofuran solution of cyclopentadiene is 1:2;
[0088] ③ Under a nitrogen atmosphere, a tetrahydrofuran solution of 1-chloropentane was added dropwise to the purple-red solution of CPD-Na within 2 hours to obtain a 1-pentyl-2,4-cyclopentadiene solution; the mass percentage of the tetrahydrofuran solution of 1-chloropentane was 8%;
[0089] The molar ratio of CPD-Na in the purple-red solution of CPD-Na to 1-chloropentane in the tetrahydrofuran solution of 1-chloropentane is 1:1.05;
[0090] ④ The solvent in the 1-pentyl-2,4-cyclopentadiene solution was extracted by decompression, and then washed with water, extracted and purified by rotary evaporation to finally obtain a light yellow oily liquid, namely 1-pentyl-2,4-cyclopentadiene. The rest is the same as in Example 1.
[0091] Example 6: This example is different from Example 2 in that the cyclopentadiene in step 1 is 1-pentyl-2,4-cyclopentadiene. The rest is the same as Example 2. The preparation method of the 1-pentyl-2,4-cyclopentadiene is the same as that described in Example 5.
[0092] Example 7: This example is different from Example 3 in that the cyclopentadiene in step 1 is 1-pentyl-2,4-cyclopentadiene. The rest is the same as Example 3. The preparation method of the 1-pentyl-2,4-cyclopentadiene is the same as that described in Example 5.
[0093] Embodiment 8: This embodiment differs from Embodiment 4 in that the cyclopentadiene in step 1 is 1-pentyl-2,4-cyclopentadiene. The rest is the same as Embodiment 4. The preparation method of the 1-pentyl-2,4-cyclopentadiene is the same as that described in Embodiment 5.
[0094] Comparative Example 1:
[0095] A method for preparing a low stress bonding adhesive material is carried out according to the following steps:
[0096] 1. Weigh 100 parts of cycloolefin copolymer resin, 0.2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 170 parts of 1-dodecene and 30 parts of cyclododecene by mass;
[0097] The 100 parts of cycloolefin copolymer resin are specifically 60 parts of cycloolefin copolymer A1 ( F4520, commercially available), 30 parts of cycloolefin copolymer A2 ( FBK80, commercially available) and 10 parts of a low molecular weight cycloolefin copolymer ( 9506F-500);
[0098] 2. Add the weighed cycloolefin copolymer resin to 1-dodecene and cyclododecene, stir for 5 hours under a nitrogen atmosphere and a temperature of 80°C, then stop heating, continue stirring, and after cooling to room temperature, add tris(2,4-di-tert-butylphenyl)phosphite, and after the tris(2,4-di-tert-butylphenyl)phosphite is dissolved, a low-stress bonding adhesive material is obtained;
[0099] Comparative Example 2: This comparative example is different from the comparative example 1 in that the 100 parts of cycloolefin copolymer resin in step 1 are specifically 50 parts of cycloolefin copolymer A1 ( F4520, commercially available), 30 parts of cycloolefin copolymer A2 ( FBK80, commercially available) and 20 parts of a low molecular weight cycloolefin copolymer ( 9506F-500). Others are the same as those in Comparative Example 1.
[0100] Comparative Example 3: This comparative example is different from the comparative example 1 in that: in step 1, the low molecular weight cycloolefin copolymer ( 9506F-500) was replaced by hydrogenated petroleum resin (Eastman Chemical Co., R1140, commercially available). Others are the same as those in Comparative Example 1.
[0101] Comparative Example 4: This comparative example is different from the comparative example 1 in that: in step 1, the low molecular weight cycloolefin copolymer ( 9506F-500) was replaced by an aliphatic hydrocarbon resin (Arakawa Chemical Company, USA, P-140, commercially available). Others are the same as those in Comparative Example 1.
[0102] Comparative Example 5: This comparative example is different from the comparative example 1 in that the 100 parts of cycloolefin copolymer resin in step 1 are specifically 65 parts of cycloolefin copolymer A1 ( F4520, commercially available), 30 parts of cycloolefin copolymer A2 ( FBK80, commercially available) and 5 parts of polyolefin elastomer (DOW, ENGAGE TM 8003, commercially available). Others are the same as those in Comparative Example 1.
[0103] Comparative Example 6: This comparative example is different from the comparative example 5 in that the polyolefin elastomer (DOW, ENGAGE TM 8003, commercially available) was replaced by a polyolefin plastomer (DOW, AFFINITY TM PL1840G, commercially available). Others are the same as those in Comparative Example 5.
[0104] Comparative Example 7: This comparative example is different from the comparative example 5 in that the polyolefin elastomer (DOW, ENGAGETM 8003, commercially available) was replaced with an α-olefin copolymer (Mitsui Chemicals, TAFMER TM A1085S, commercially available). Others are the same as those in Comparative Example 5.
[0105] Comparative Example 8: This comparative example is different from the comparative example 1 in that: in step 1, the low molecular weight cycloolefin copolymer ( 9506F-500) was replaced by polycarbonate (COVESTRO, 2807, commercially available). Others are the same as those in Comparative Example 1.
[0106] Comparative Example 9: This comparative example is different from the comparative example 1 in that: in step 1, the low molecular weight cycloolefin copolymer ( 9506F-500) was replaced with general-purpose polystyrene (Shanghai Secco Petrochemical Co., Ltd., GPPS-123P, commercially available). Others were the same as those in Comparative Example 1.
[0107] Comparative Example 10: This comparative example is different from Comparative Example 5 in that the 100 parts of cycloolefin copolymer resin in step 1 are specifically 65 parts of cycloolefin copolymer A1 ( F4520, commercially available), 30 parts of cycloolefin copolymer A2 ( FBK80, commercially available), 4 parts of bisphenol A epoxy resin (Nantong Xingchen Synthetic Materials Co., Ltd., E-51, commercially available) and 1 part of 4,4-diaminophenylsulfone (TCI reagent, AR, commercially available). Others are the same as those in Comparative Example 5.
[0108] The low stress bonding adhesive materials prepared in Examples 1 to 8 and Comparative Examples 1 to 10 were tested for solubility, adhesive layer state after bonding, chip shear strength, high temperature stability, residual stress, and cleanability. The detailed evaluation method is as follows:
[0109] 1. Solubility: Visually observe whether the low-stress bonding adhesive material is uniform and clear after being placed at room temperature for 0h, 12h, 24h, 48h, 7days, and 30days.
[0110] 2. State of the adhesive layer after bonding: Spin-coat the low-stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters, ensuring that the adhesive layer thickness is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Then use a wafer bonder to bond the silicon wafer to the quartz carrier wafer, with bonding parameters of 200℃ / 2min and 0.05MPa. After bonding, observe whether the adhesive layer is homogeneous and has no obvious defects under a microscope.
[0111] 3. Chip shear strength: Spin-coat the low-stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters, ensuring that the adhesive layer thickness is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Place a 2mm×2mm silicon wafer on the above silicon wafer and heat and cure it on a baking plate at 200℃ / 2min. Use a chip push-pull force tester (NordsonDage 3800) to perform compression shear tests on the samples. The sample test temperatures are 25℃, 100℃, 150℃, 200, and 250℃, respectively, and the shear rate is 100μm / s.
[0112] 4. High temperature stability: Spin-coat the low stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters, ensuring that the thickness of the adhesive layer is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Then use a wafer bonder to bond the silicon wafer to the quartz carrier wafer, with bonding parameters of 200℃ / 2min and 0.05MPa. After bonding, place the sample on a baking plate and treat it with conditions of 250℃ / 30min, 250℃ / 120min, 300℃ / 30min, 300℃ / 120min, 350℃ / 30min, 350℃ / 120min, etc., and observe whether there are any defects under a microscope after treatment.
[0113] 5. Residual stress test: Spin-coat the low-stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters, ensuring that the adhesive layer thickness is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Put the sample into a residual stress tester (TOHO FLX2320-S) for testing, and test the residual stress value accumulated by the sample after being treated at 250℃ / 30min, 250℃ / 120min, 300℃ / 30min, and 300℃ / 120min and then returning to room temperature.
[0114] 6. Cleanability test: Spin-coat the low-stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters, ensuring that the thickness of the adhesive layer is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Then use a wafer bonder to bond the silicon wafer to the quartz carrier wafer, with bonding parameters of 200℃ / 2min and 0.05MPa. After bonding, place it on a 250℃ heating plate and manually slide the two wafers horizontally until they are completely separated. Use a specific solvent to clean the two separated samples separately. The above process is to simulate the process of the bonding adhesive material during the bonding and debonding process, so as to verify that the bonding adhesive material can still be cleaned after the degree of cross-linking increases after being heated. The specific cleaning steps are shown in Table 1 below. After cleaning, observe the surface of the wafer under a microscope to see if there is any residue.
[0115] Table 1
[0116]
[0117] In step 1 of the table, 1-dodecene was added dropwise for 10 seconds at a spin coating speed of 600 rpm and a dripping speed of 1 ml / s. In step 4, isopropanol was added dropwise for 5 seconds at a spin coating speed of 1000 rpm and a dripping speed of 1 ml / s.
[0118] 7. Medium resistance test: Spin the low stress bonding adhesive material on a 4-inch silicon wafer with appropriate process parameters to ensure that the thickness of the adhesive layer is 30μm±1μm after drying the solvent, and the drying process is 120℃ / 5min+180℃ / 3min. Then use a wafer bonder to bond the silicon wafer to the quartz carrier wafer, with bonding parameters of 200℃ / 2min and 0.05MPa. After bonding, soak them in different media under certain conditions, and then observe whether the two wafers of the sample are debonded or slipped, and whether the bonding layer at the edge of the wafer is intact. If there is no debonding or slipping between the two wafers, and the bonding layer at the edge of the wafer is intact, it is judged as A; if there is debonding or slipping between the two wafers, it is judged as B; if the bonding layer at the edge of the wafer is incomplete, it is judged as C; if there is debonding or slipping between the two wafers, and the bonding layer at the edge of the wafer is incomplete, it is judged as D.
[0119] Table 2
[0120]
[0121]
[0122] “—” in the table means that this test was not performed.
[0123] Table 3
[0124]
[0125] “—” in the table means that this test was not performed.
[0126] Table 4
[0127]
[0128]
[0129] “—” in the table indicates that the value is lower than the lower limit of the equipment test.
[0130] Table 5
[0131]
[0132] Table 6
[0133]
[0134]
[0135] Compared with Comparative Examples 5 to 10, Examples 1 to 8 are as follows:
[0136] Compared with conventional elastomers and thermoplastic resins, cyclopentadiene can be more compatible with cycloolefin copolymers in specific solvent systems and remain stable. The polycyclopentadiene formed after a certain degree of cross-linking of cyclopentadiene can also exist uniformly with the cycloolefin copolymer in the system and can still be washed by specific solvents, which is significantly better than conventional thermosetting resins.
[0137] Compared with Comparative Examples 1 to 4, Examples 1 to 8 are as follows:
[0138] 1. It has better high-temperature stability. After high-temperature treatment under different conditions, the adhesive layer has basically no defects, indicating that cyclopentadiene can well improve the high-temperature stability of cycloolefin copolymers. The temporary bonding adhesive material prepared by the present invention has higher temperature resistance.
[0139] 2. The chip shear strength is generally high, especially the shear strength at high temperature, which indicates that the cross-linked structure of polycyclopentadiene greatly improves the strength of the system, so that the temporary bonding adhesive material described in the present invention has better high-temperature strength.
[0140] 3. The residual stress value after heat treatment is low, especially after treatment at a higher temperature, the residual stress value can still be maintained at a low level, which indicates that the cross-linked structure of polycyclopentadiene has an obvious toughening effect, so that the temporary bonding adhesive material described in the present invention has the characteristics of low stress.
[0141] 4. Excellent media resistance, can withstand common wafer processing reagents and conditions.
[0142] Figure 1 This is the infrared spectrum of 1-pentyl-2,4-cyclopentadiene prepared in Example 5. As can be seen from the figure, 2943cm -1 、2921cm -1 、2866cm -1 and 2852cm -1 There are absorption peaks at four wave numbers, which belong to the -CH2- stretching vibration absorption peak in the norbornene structural unit, 1456cm -1 The characteristic peaks of -CH2- shear vibration on the pentyl group indicate that cyclopentadiene monomer has been synthesized.
Claims
1. A low stress bonding adhesive material, characterized in that It is prepared from 100 parts of cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant and 100 to 250 parts of a solvent in parts by mass. The cyclopentadiene is dicyclopentadiene or 1-pentyl-2,4-cyclopentadiene; The structural formula of the dicyclopentadiene is The structural formula of the 1-pentyl-2,4-cyclopentadiene is The catalyst is one of trinonylphenol tungsten trichloride, diethylaluminum monochloride, ethylaluminum dichloride, diisobutylaluminum chloride, methylaluminum dichloride and dimethylaluminum chloride, or a mixture of several of them.
2. A low stress bonding adhesive material according to claim 1, characterized in that The weight average molecular weight of the cycloolefin copolymer resin is 50,000 to 300,000, and the glass transition temperature is above 80°C.
3. A low stress bonding adhesive material according to claim 1, characterized in that The antioxidant is a phenolic antioxidant or a phosphite antioxidant.
4. The low stress bonding adhesive material according to claim 1, characterized in that The antioxidant is one of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and tris(2,4-di-tert-butylphenyl) phosphite or a mixture of both.
5. The low stress bonding adhesive material according to claim 1, characterized in that The boiling point of the solvent is 100°C to 230°C.
6. A low stress bonding adhesive material according to claim 5, characterized in that The solvent is dipentene, 1-dodecene, cyclododecene, pinene, dicyclohexene, cyclooctane, cyclopentane, cycloheptane, butanone, cyclohexanone, cyclopentanone, D-limonene or butylcyclohexane.
7. The low stress bonding adhesive material according to claim 1, characterized in that The 1-pentyl-2,4-cyclopentadiene is specifically prepared according to the following steps: ①Heat dicyclopentadiene to 140℃~180℃, collect the fraction at 37℃~42℃ to obtain liquid cyclopentadiene, and seal and store the liquid cyclopentadiene in a low temperature environment below 0℃ for future use; ② Using tetrahydrofuran to dissolve liquid cyclopentadiene to obtain a tetrahydrofuran solution of cyclopentadiene; Under nitrogen protection, tetrahydrofuran is added to NaH to dissolve it to obtain a reaction system. Under ice bath conditions, the reaction system is kept at 0°C. Under the condition of a dropwise addition rate of 0.5 mL / s to 1 mL / s, a tetrahydrofuran solution of cyclopentadiene is slowly added dropwise to the reaction system. The reaction is carried out for 4 h to 6 h to obtain a purple-red solution of CPD-Na, which is then sealed and stored at low temperature for later use. The mass ratio of NaH in the reaction system to cyclopentadiene in the tetrahydrofuran solution of cyclopentadiene is 1:(2-2.5); ③ Under nitrogen atmosphere, add the tetrahydrofuran solution of 1-chloropentane dropwise into the purple-red solution of CPD-Na over 2 to 4 hours to obtain a solution of 1-pentyl-2,4-cyclopentadiene; The molar ratio of CPD-Na in the purple-red solution of CPD-Na to 1-chloropentane in the tetrahydrofuran solution of 1-chloropentane is 1:(1-1.1); ④ Extract the solvent from the 1-pentyl-2,4-cyclopentadiene solution by reducing pressure, then wash with water, extract and purify by rotary evaporation, and finally obtain a light yellow oily liquid, namely 1-pentyl-2,4-cyclopentadiene; The mass percentage of the tetrahydrofuran solution of cyclopentadiene described in step ② is 10% to 20%; the mass percentage of NaH in the reaction system described in step ② is 5% to 15%; the mass percentage of the tetrahydrofuran solution of 1-chloropentane described in step ③ is 8% to 15%.
8. The low stress bonding adhesive material according to claim 1, characterized in that The cyclopentadiene premixed with the catalyst is specifically prepared according to the following steps: 100 parts of cyclopentadiene, 0.05 parts to 0.2 parts of the catalyst and 240 parts to 400 parts of chloroform solution are weighed by mass, the weighed cyclopentadiene is added to the chloroform solution, and then the catalyst is added, stirred at room temperature for 1 hour to 4 hours, and the chloroform solution is removed by reduced pressure distillation to obtain the cyclopentadiene premixed with the catalyst.
9. The method for preparing a low stress bonding adhesive material according to claim 1, characterized in that It is carried out in the following steps:
1. Weigh 100 parts of cycloolefin copolymer resin, 2 to 10 parts of cyclopentadiene premixed with a catalyst, 0.1 to 0.5 parts of an antioxidant, and 100 to 250 parts of a solvent by mass; 2. Add the weighed cycloolefin copolymer resin to the solvent, stir for 4h to 6h under a nitrogen atmosphere and a temperature of 50℃ to 120℃, then stop heating and continue stirring. After cooling to room temperature, add an antioxidant. After the antioxidant is dissolved, add the cyclopentadiene premixed with the catalyst at a feeding time of 30min to 90min, and continue stirring at room temperature for 1h to 4h to obtain a low stress bonding adhesive material.