Carbon nanotube catalyst based on zeolite imidazolate framework and preparation method and application thereof
By employing a simplified method for preparing zeolite imidazole ester framework carbon nanotube catalysts, the problem of metal nanoparticle aggregation was solved, enabling efficient and low-cost carbon nanotube growth and improving the performance of supercapacitors.
Patent Information
- Application Number
- CN202310256104.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-16
AI Technical Summary
Existing zeolite imidazole ester framework catalysts are prone to agglomeration of metal nanoparticles and carbon skeletons during high-temperature pyrolysis, resulting in the performance of carbon nanotube-based electronic devices falling short of expectations. Furthermore, traditional preparation methods are complex and costly.
A carbon nanotube catalyst based on a zeolite imidazole ester framework was prepared by heating melamine foam with metal salt and imidazole solution under an inert atmosphere to form a uniform zeolite imidazole ester framework composite material, followed by secondary heating to form a carbon nanotube catalyst. This method simplifies the preparation process and inhibits the aggregation of metal nanoparticles.
A simplified fabrication process was achieved, reducing costs. Furthermore, the specific surface area and conductivity of the supercapacitor were improved through uniformly grown carbon nanotube catalysts, enhancing charge transport capabilities and improving device performance.
Smart Images

Figure CN116328750B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy storage devices, and in particular to a carbon nanotube catalyst based on a zeolite imidazolate framework, and a preparation method and application thereof. Background Art
[0002] In order to solve the increasingly serious energy problem, it is urgent to vigorously develop energy conversion systems based on clean and renewable energy. However, the use of these new energy sources is limited by natural conditions. For example, hydropower and wind power are limited by geographical location, while solar energy is limited by geographical location and time. Therefore, it is particularly important to develop efficient energy storage devices. Supercapacitors have become a research hotspot in current energy storage electronic devices because of their excellent characteristics such as large current fast charging and discharging characteristics, long cycle life, safety and reliability.
[0003] As a typical one-dimensional carbon nanomaterial, carbon nanotubes have the advantages of large specific surface area, excellent electrical conductivity and electrochemical stability, and are widely used in the research of supercapacitor electrode materials. At present, chemical vapor deposition has become the most commonly used method for synthesizing carbon nanotubes in recent years due to its advantages such as low cost and easy control of experimental parameters. However, this method requires the use of electron beam evaporation coating technology with strict operation, complex process, high energy consumption and high cost to evaporate the catalyst on the substrate surface, which seriously restricts the development and application of carbon nanotubes.
[0004] Recently, some researchers have reported a zeolite imidazolate framework material that is self-assembled by metal-ligand complexation between organic ligands and metal ions. Because it has abundant nitrogen-containing groups, it can obtain nitrogen-doped porous carbon after high-temperature pyrolysis, and can also form chemical bonds with non-precious metals, making it an ideal choice for growing carbon nanotube catalysts. Most of the zeolite imidazolate framework catalysts reported so far are prone to serious agglomeration of metal nanoparticles and carbon skeletons during high-temperature pyrolysis, resulting in the performance of the constructed carbon nanotube-based electronic devices failing to meet expectations.
[0005] Patent CN110844899A discloses a carbon nanotube composite cobalt sulfide nanomaterial and its preparation method and application. The zeolite imidazolate framework of the patent is obtained by mixing cobalt salt solution, zinc salt solution and 2-methylimidazole solution evenly, reacting to obtain a precipitate, washing and drying, and calcining the zeolite imidazolate framework structure material under an inert atmosphere to obtain a carbon nanotube composite metal cobalt nanomaterial. However, the patent has the following defects: the zeolite imidazolate framework catalyst with a dodecahedral structure obtained by the patent is in powder form and needs to be mixed with a conductive agent and a binder and coated on a current collector before it can be used as an electrode material for the device. The preparation process is complicated, and the addition of a conductive agent and a binder will reduce the performance of the device.
[0006] Therefore, the key to developing carbon nanotube-based flexible electronic devices is to prepare carbon nanotubes with optimal performance by designing a reasonable zeolite imidazolate framework catalyst structure. Summary of the invention
[0007] The purpose of the present invention is to overcome the defects of the above-mentioned prior art zeolite imidazolate framework catalyst, such as the serious agglomeration of metal nanoparticles and carbon skeleton during high-temperature pyrolysis, and to provide a carbon nanotube catalyst based on zeolite imidazolate framework and its preparation method and application.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] One of the technical solutions of the present invention is to provide a method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework, comprising the following steps:
[0010] S1, heating carbonized melamine foam once in an inert gas atmosphere to obtain melamine carbon foam;
[0011] S2, mixing the cobalt nitrate hexahydrate aqueous solution and the 2-methylimidazole aqueous solution at room temperature to obtain a mixed solution;
[0012] S3, immersing the melamine carbon foam obtained in step S1 into the mixed solution obtained in step S2 to react at room temperature to obtain a melamine carbon foam / zeolite imidazole framework composite material;
[0013] S4, reheating and carbonizing the melamine carbon foam / zeolite imidazolate framework composite material obtained in step S3 under an inert gas atmosphere to obtain a carbon nanotube catalyst based on the zeolite imidazolate framework.
[0014] Furthermore, in steps S1 and S4, the inert gas is argon.
[0015] Furthermore, in step S1, the flow rate of argon gas is 300-400 sccm; in step S4, the flow rate of argon gas is 50-100 sccm.
[0016] Furthermore, in step S1, the temperature of the primary heating carbonization is 500-600° C., and the time of the primary heating carbonization is 1-4 hours.
[0017] Furthermore, in step S2, the concentration of the cobalt nitrate hexahydrate aqueous solution is 1-3 mmol / L, and the concentration of the 2-methylimidazole aqueous solution is 12-20 mmol / L; the mixing and stirring speed is 1000-1400 rpm, and the mixing and stirring time is 1-3 min.
[0018] Furthermore, in step S3, the reaction time at room temperature is 6 to 12 hours.
[0019] Furthermore, in step S4, the temperature of the secondary heating carbonization is 300 to 450° C., and the time of the secondary heating carbonization is 1 to 3 hours.
[0020] The second technical solution of the present invention is to provide a carbon nanotube catalyst based on a zeolite imidazolate framework, based on the preparation method described in one of the above technical solutions.
[0021] Furthermore, the particle size of the carbon nanotube catalyst is 1 to 5 μm.
[0022] The third technical solution of the present invention is to provide an application of the carbon nanotube catalyst based on the zeolite imidazolate framework as described above, wherein the carbon nanotube catalyst is applied in the field of supercapacitors.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The carbon nanotube catalyst based on the zeolite imidazolate framework of the present invention is synthesized by a simple solution method. Compared with the traditional evaporation coating method with high energy consumption and complicated process, this method has the advantages of simple process and low cost;
[0025] (2) The supercapacitor prepared by the carbon nanotube catalyst based on the zeolite imidazolate framework of the present invention has a high area specific capacity of 541.0 mF cm -2 The zeolite imidazolate framework nanosheets in the carbon nanotube catalyst based on the zeolite imidazolate framework are uniformly grown on the melamine carbon foam skeleton, which can effectively inhibit the agglomeration of cobalt nanoparticles and the carbon skeleton and further increase the specific surface area of the material; in addition, the good interface bonding between the functional components of the composite material is conducive to promoting the transmission of charges or ions between the interfaces.
[0026] (3) The electrode material of this patent is based on carbon foam, and no additional conductive agent and binder are required; in addition, the obtained zeolite imidazolate framework catalyst belongs to a two-dimensional layered nanosheet structure, which forms a three-dimensional network structure with the subsequently grown carbon nanotubes. This structure has a larger specific surface area, promotes the transmission of charges or ions, shortens the migration path of charges or ions, and increases the conductivity of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the preparation process of the carbon nanotube catalyst based on the zeolite imidazolate framework and the melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material of the present invention.
[0028] Figure 2 This is a low-magnification scanning electron microscope photograph of the carbon nanotube catalyst based on the zeolite imidazolate framework prepared in Example 1.
[0029] Figure 3 This is a high-magnification scanning electron microscope photograph of the carbon nanotube catalyst based on the zeolite imidazolate framework prepared in Example 1.
[0030] Figure 4 This is a low-magnification scanning electron microscope photograph of the cross section of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared in Example 1.
[0031] Figure 5 This is a high-magnification scanning electron microscope photograph of the cross section of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared in Example 1.
[0032] Figure 6 This is a low-magnification transmission electron microscope photograph of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared in Example 1.
[0033] Figure 7 This is a high-magnification transmission electron microscope photograph of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared in Example 1.
[0034] Figure 8 This is a low-magnification scanning electron microscope photograph of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1.
[0035] Fig. 9 This is a high-magnification scanning electron microscope photograph of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1.
[0036] Fig.10 These are X-ray diffraction patterns of the melamine carbon foam, melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material, and melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1.
[0037] Fig.11 These are Raman spectra of the melamine carbon foam, melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material, and melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1.
[0038] Fig.12 Cyclic voltammetry curves of the supercapacitor based on melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1 at different electrodeposition times.
[0039] Fig.13The constant current charge-discharge curves of the supercapacitor based on the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1 at different electrodeposition times.
[0040] Fig.14 Impedance spectra of the supercapacitor based on melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1 at different electrodeposition times.
[0041] Fig.15 This is a curve showing the variation of the area specific capacity of the supercapacitor based on the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material prepared in Example 1 at different electrodeposition times as a function of deposition time. DETAILED DESCRIPTION
[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0043] In the following examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.
[0044] Embodiment 1:
[0045] A method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework, the preparation process diagram is as follows Figure 1 As shown, the specific steps include:
[0046] (1) heating and carbonizing the melamine foam, with an argon flow rate of 300 sccm, a temperature of 500° C., and a carbonization time of 3 h to obtain a melamine carbon foam;
[0047] (2) mixing 1 mmol / L aqueous solution of cobalt nitrate hexahydrate and 12 mmol / L aqueous solution of 2-methylimidazole at 1000 rpm for 3 min;
[0048] (3) immersing the melamine carbon foam obtained in step (1) into the mixed solution of step (2), and reacting for 12 hours at room temperature to obtain a melamine carbon foam / zeolite imidazole framework composite material;
[0049] (4) heating and carbonizing the melamine carbon foam / zeolite imidazolate framework composite material obtained in step (3) at an argon flow rate of 50 sccm, a temperature of 300° C., and a carbonization time of 3 h to obtain a carbon nanotube catalyst based on a zeolite imidazolate framework;
[0050] The prepared carbon nanotube catalyst based on zeolite imidazolate framework is used to grow carbon nanotubes. The synthesis method of the carbon nanotubes is a chemical vapor deposition method, with the carbon nanotube catalyst as a matrix, ethylene as a carbon source, and a mixed gas of argon and hydrogen as a carrier gas, wherein the flow rates of argon, hydrogen and ethylene are 300-600sccm, 40-100sccm and 40-80sccm respectively, the growth temperature range is 750-900°C, and the growth time is 15-60min.
[0051] A supercapacitor was assembled using melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material as electrodes, filter paper as a separator, and polyvinyl alcohol / lithium chloride hydrogel system as an electrolyte.
[0052] The synthesis method of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite electrode is an electrochemical deposition method, using melamine carbon foam / zeolite imidazolate framework / carbon nanotube as raw materials, and a mixed solution of manganese sulfate, sodium acetate, ethanol and water as electrolyte (wherein the concentration of manganese sulfate is 60 mg / mL, the concentration of sodium acetate is 30 mg / mL, and the volume ratio of ethanol to water is 1:9), the raw materials are placed in the electrolyte at 0.3 mA / cm 2 The reaction was carried out at a constant current density of 1.5-2.5 for 15-35 min to obtain a melamine carbon foam / zeolite imidazole framework / carbon nanotube / manganese dioxide composite electrode.
[0053] The preparation method of the polyvinyl alcohol / lithium chloride hydrogel system electrolyte is as follows: lithium chloride is added into water to dissolve, the concentration of lithium chloride is 0.04-0.2 g / mL, then polyvinyl alcohol is dissolved in the above-mentioned mixed solution, wherein the concentration of polyvinyl alcohol is 0.04-0.2 g / mL, and stirred at a temperature of 75-85°C for 10-30 hours until it becomes clear.
[0054] The specific test results of this embodiment are as follows:
[0055] Figure 2 and Figure 3 This is a scanning electron microscope photo of a carbon nanotube catalyst based on a zeolite imidazolate framework. The carbon nanotube catalyst is a melamine carbon foam / zeolite imidazolate framework (CF / ZIFs) composite material. It can be seen that the zeolite imidazolate framework nanosheet array is uniformly grown on the melamine carbon foam skeleton, and the carbon nanotube catalyst maintains an intact nanosheet structure after high-temperature carbonization.
[0056] Figure 4 and Figure 5This is a cross-sectional scanning electron microscope photograph of a melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared using a carbon nanotube catalyst based on a zeolite imidazolate framework. It can be seen that the carbon nanotubes form a fully entangled network structure on the surface of the zeolite imidazolate framework material, which is beneficial to the transmission of electrons and ions, and reduces the adverse effects of volume changes.
[0057] Figure 6 and Figure 7 This is a transmission electron microscope photograph of a melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material prepared based on a carbon nanotube catalyst of a zeolite imidazolate framework. As can be seen from the figure, the carbon nanotube has a bamboo-like structure with an outer diameter of about 11 nm.
[0058] Figure 8 and Fig. 9 This is a scanning electron microscope photograph of a melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material. It can be clearly seen that manganese dioxide nanosheets grow on the surface of carbon nanotubes prepared by a carbon nanotube catalyst based on a zeolite imidazolate framework.
[0059] Fig.10 The X-ray diffraction patterns of melamine carbon foam (CF), melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite material (CNTs@CF) and melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material (MnO2 / CNTs@CF) show typical diffraction peaks of carbon nanotubes (CNTs), cobalt-zeolite imidazolate framework and manganese dioxide, indicating that the zeolite imidazolate framework is a catalyst for growing carbon nanotubes and is well composited with manganese dioxide.
[0060] Fig.11 The Raman scattering spectra of melamine carbon foam (CF), melamine carbon foam / zeolite imidazolate framework / carbon nanotube composite (CNTs@CF) and melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite (MnO2 / CNTs@CF) are shown in Figure 1. The Raman characteristic peak of carbon nanotubes appears at 1360 cm -1 and 1586cm -1 The Raman peak of the zeolite imidazolate framework is located at 666 cm -1 , which corresponds to the vibration of cobalt / cobalt oxide. The melamine carbon foam / zeolite imidazolate framework / carbon nanotubes / manganese dioxide composite has characteristic peaks of pure carbon nanotubes and manganese dioxide, which again indicates that manganese dioxide is well composited with carbon nanotubes.
[0061] The key technical indicators of the electrochemical performance of supercapacitors include specific capacity, energy density, power density and long-term stability, which are mainly characterized by cyclic voltammetry (CV), constant current charge-discharge method and impedance spectrum. Among them, specific capacity is the most important parameter for representing the charge energy stored by supercapacitors. According to the constant current charge-discharge curve of the capacitor, the area specific capacity (C S ) is calculated by the following formula:
[0062] C S =IΔt / SΔV,
[0063] where I, S, ΔV and Δt are discharge current, effective electrode area, voltage window and discharge time, respectively.
[0064] Fig.12 Supercapacitors based on melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composites with different deposition times at a scan rate of 100 mV s -1 All CV curves maintain good rectangular features, indicating that the device has ideal double-layer capacitance properties.
[0065] Fig.13 The figure shows the charge and discharge curves of supercapacitors based on melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite materials with different deposition times at a constant current of 0.1 mA, where the voltage range is 0-1.0 V. It can be seen that the constant current charge and discharge curves are basically symmetrical triangles, showing typical supercapacitor characteristics.
[0066] Fig.14 The Nyquist plot of supercapacitors based on melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composites with different deposition times. The low-frequency curve is upright, showing pure capacitance behavior. The high-frequency region shows that as the deposition time of manganese dioxide in the composite increases, the series resistance of the device increases, which is caused by the low conductivity of manganese dioxide.
[0067] Fig.15 The relationship between the area specific capacity and deposition time of the supercapacitor based on the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material with different deposition times was calculated in detail. The results showed that when the manganese dioxide deposition time was 35 min, the C of the supercapacitor was S The highest value (541.0mF cm -2 ), when only carbon nanotube electrode materials are used under the same conditions (19.2mF cm -2 ). Overall, the device reduces the difficulty and cost of preparation while increasing the capacity of the capacitor, and has good application prospects.
[0068] Embodiment 2:
[0069] A method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework, the preparation process diagram is as follows Figure 1 As shown, the specific steps include:
[0070] (1) carbonizing the melamine foam at an argon flow rate of 400 sccm, a temperature of 600° C., and a carbonization time of 1 h to obtain a melamine carbon foam;
[0071] (2) mixing 1 mmol / L aqueous solution of cobalt nitrate hexahydrate and 12 mmol / L aqueous solution of 2-methylimidazole at 1400 rpm for 3 min;
[0072] (3) immersing the melamine carbon foam obtained in step (1) into the above-mentioned mixed solution, and reacting for 6 hours at room temperature to obtain a melamine carbon foam / zeolite imidazole framework composite material;
[0073] (4) carbonizing the melamine carbon foam / zeolite imidazolate framework composite material obtained in step (3) at an argon flow rate of 100 sccm, a temperature of 450° C., and a carbonization time of 3 h to obtain a carbon nanotube catalyst based on a zeolite imidazolate framework;
[0074] The prepared carbon nanotube catalyst based on zeolite imidazolate framework is used to grow carbon nanotubes. The synthesis method of the carbon nanotubes is a chemical vapor deposition method, with the carbon nanotube catalyst as a matrix, ethylene as a carbon source, and a mixed gas of argon and hydrogen as a carrier gas, wherein the flow rates of argon, hydrogen and ethylene are 300-600sccm, 40-100sccm and 40-80sccm respectively, the growth temperature range is 750-900°C, and the growth time is 15-60min.
[0075] A supercapacitor was assembled using melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material as electrodes, filter paper as a separator, and polyvinyl alcohol / lithium chloride hydrogel system as an electrolyte.
[0076] The synthesis method of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite electrode is an electrochemical deposition method, using melamine carbon foam / zeolite imidazolate framework / carbon nanotube as raw materials, and a mixed solution of manganese sulfate, sodium acetate, ethanol and water as electrolyte (wherein the concentration of manganese sulfate is 60 mg / mL, the concentration of sodium acetate is 30 mg / mL, and the volume ratio of ethanol to water is 1:9), the raw materials are placed in the electrolyte at 0.3 mA / cm 2 The reaction was carried out at a constant current density of 1.5-2.5 for 15-35 min to obtain a melamine carbon foam / zeolite imidazole framework / carbon nanotube / manganese dioxide composite electrode.
[0077] The preparation method of the polyvinyl alcohol / lithium chloride hydrogel system electrolyte is as follows: lithium chloride is added into water to dissolve, the concentration of lithium chloride is 0.04-0.2 g / mL, then polyvinyl alcohol is dissolved in the above-mentioned mixed solution, wherein the concentration of polyvinyl alcohol is 0.04-0.2 g / mL, and stirred at a temperature of 75-85°C for 10-30 hours until it becomes clear.
[0078] The test results show that the capacitor obtained in this embodiment has excellent characteristics such as large current rapid charging and discharging characteristics, safety and reliability.
[0079] Embodiment 3:
[0080] A method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework, the preparation process diagram is as follows Figure 1 As shown, the specific steps include:
[0081] (1) carbonizing the melamine foam at an argon flow rate of 400 sccm, a temperature of 500° C., and a carbonization time of 1 h to obtain a melamine carbon foam;
[0082] (2) mixing 1 mmol / L aqueous solution of cobalt nitrate hexahydrate and 12 mmol / L aqueous solution of 2-methylimidazole at 1000 rpm for 3 min;
[0083] (3) immersing the melamine carbon foam obtained in step (1) into the above-mentioned mixed solution and reacting for 8 hours at room temperature to obtain a melamine carbon foam / zeolite imidazole framework composite material;
[0084] (4) carbonizing the melamine carbon foam / zeolite imidazolate framework composite material obtained in step (3) at an argon flow rate of 50 sccm, a temperature of 300° C., and a carbonization time of 2 h to obtain a carbon nanotube catalyst based on a zeolite imidazolate framework;
[0085] The prepared carbon nanotube catalyst based on zeolite imidazolate framework is used to grow carbon nanotubes. The synthesis method of the carbon nanotubes is a chemical vapor deposition method, with the carbon nanotube catalyst as a matrix, ethylene as a carbon source, and a mixed gas of argon and hydrogen as a carrier gas, wherein the flow rates of argon, hydrogen and ethylene are 300-600sccm, 40-100sccm and 40-80sccm respectively, the growth temperature range is 750-900°C, and the growth time is 15-60min.
[0086] A supercapacitor was assembled using melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite material as electrodes, filter paper as a separator, and polyvinyl alcohol / lithium chloride hydrogel system as an electrolyte.
[0087] The synthesis method of the melamine carbon foam / zeolite imidazolate framework / carbon nanotube / manganese dioxide composite electrode is an electrochemical deposition method, using melamine carbon foam / zeolite imidazolate framework / carbon nanotube as raw materials, and a mixed solution of manganese sulfate, sodium acetate, ethanol and water as electrolyte (wherein the concentration of manganese sulfate is 60 mg / mL, the concentration of sodium acetate is 30 mg / mL, and the volume ratio of ethanol to water is 1:9), the raw materials are placed in the electrolyte at 0.3 mA / cm 2 The reaction was carried out at a constant current density of 1.5-2.5 for 15-35 min to obtain a melamine carbon foam / zeolite imidazole framework / carbon nanotube / manganese dioxide composite electrode.
[0088] The preparation method of the polyvinyl alcohol / lithium chloride hydrogel system electrolyte is as follows: lithium chloride is added into water to dissolve, the concentration of lithium chloride is 0.04-0.2 g / mL, then polyvinyl alcohol is dissolved in the above-mentioned mixed solution, wherein the concentration of polyvinyl alcohol is 0.04-0.2 g / mL, and stirred at a temperature of 75-85°C for 10-30 hours until it becomes clear.
[0089] The test results show that the capacitor obtained in this embodiment has excellent characteristics such as large current rapid charging and discharging characteristics, safety and reliability.
[0090] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework, characterized in that: The steps include: S1, heating carbonized melamine foam once in an inert gas atmosphere to obtain melamine carbon foam; S2, mixing the cobalt nitrate hexahydrate aqueous solution and the 2-methylimidazole aqueous solution at room temperature to obtain a mixed solution; S3, immersing the melamine carbon foam obtained in step S1 into the mixed solution obtained in step S2 to react at room temperature to obtain a melamine carbon foam / zeolite imidazole framework composite material; S4, reheating and carbonizing the melamine carbon foam / zeolite imidazolate framework composite material obtained in step S3 under an inert gas atmosphere to obtain a carbon nanotube catalyst based on the zeolite imidazolate framework; Wherein, in steps S1 and S4, the inert gas is argon; In step S1, the argon gas flow rate is 300-400 sccm; in step S4, the argon gas flow rate is 50-100 sccm; In step S1, the temperature of the primary heating carbonization is 500-600°C, and the time of the primary heating carbonization is 1-4h; In step S4, the temperature of the secondary heating carbonization is 300 to 450° C., and the time of the secondary heating carbonization is 1 to 3 hours.
2. The method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework according to claim 1, characterized in that: In step S2, the concentration of the cobalt nitrate hexahydrate aqueous solution is 1-3 mmol / L, and the concentration of the 2-methylimidazole aqueous solution is 12-20 mmol / L; the mixing and stirring speed is 1000-1400 rpm, and the mixing and stirring time is 1-3 min.
3. The method for preparing a carbon nanotube catalyst based on a zeolite imidazolate framework according to claim 1, characterized in that: In step S3, the reaction time at room temperature is 6 to 12 hours.
4. A carbon nanotube catalyst based on a zeolite imidazolate framework, characterized in that: It is prepared based on the preparation method described in any one of claims 1 to 3.
5. The carbon nanotube catalyst based on zeolite imidazolate framework according to claim 4, characterized in that: The particle size of the carbon nanotube catalyst is 1 to 5 μm.
6. An application of the carbon nanotube catalyst based on the zeolite imidazolate framework as claimed in claim 4, characterized in that: The carbon nanotube catalyst is applied in the field of supercapacitors.