Preparation method of carbon fiber thermal conductive pad

By baking carbon fiber thermal gaskets in the mold, using the shear force of the expansion agent to drive the directional arrangement of carbon fibers, the problem that traditional thermal gaskets cannot meet the thermal conductivity needs of high-power electronic devices is solved, and high thermal conductivity and simplification are achieved The dual effect of craftsmanship.

CN116330694BActive Publication Date: 2024-11-22SHENZHEN HFC SHIELDING PRODS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310492860.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-22
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

Traditional thermal conductivity gaskets cannot meet the high thermal conductivity needs of high power and high-density electronic devices, especially in chip operation in the 5G era, traditional silicone thermal conductivity gaskets cannot meet the chip's temperature management requirements.

Method used

Using a preparation method of carbon fiber thermal gasket, the carbon fiber, adhesive material and expansion agent are filled in the mold of the variable cavity, and the expansion agent is heated to expand the expansion agent to generate shear force, thereby driving the direction of the carbon fiber. Arrange to achieve improved thermal conductivity, and at the same time complete vulcanization during a baking process, simplifying process steps.

Benefits of technology

The high thermal conductivity coefficient of carbon fiber thermal gasket is achieved, reaching 600 W/m·K~1200 W/m·K, which meets the thermal conductivity requirements of high-power electronic devices, simplifies the preparation process, reduces steps and improves efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116330694B_ABST
    Figure CN116330694B_ABST
Patent Text Reader

Abstract

The present application relates to the field of thermal conductive materials, and specifically, to a method for preparing a carbon fiber thermal conductive gasket. Fill the mold cavity with a mixture of carbon fiber, adhesive, and expansion agent; the volume of the mold cavity is variable, and the cavity is formed by an immovable first wall and a movable second wall; the second wall can be moved along the X-axis; the mold is baked so that the expansion agent in the mixture expands due to heat and generates a shear force acting on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves along the X-axis, driving the carbon fibers in the mixture to be oriented. The method for preparing a carbon fiber thermal conductive gasket provided in the present application can cure and vulcanize the adhesive at the same time as baking, thereby reducing the preparation steps and improving efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of thermal conductive materials, and in particular to a method for preparing a carbon fiber thermal conductive gasket. Background Art

[0002] Since the advent of the 5G era, integrated circuits have become increasingly dense, chip operating frequencies have become higher and higher, and there are more and more heat-generating devices, which have placed extremely stringent requirements on thermal conductivity. Traditional thermal conductivity solutions can no longer meet the requirements, especially for core components such as chips. In order to achieve operating processing capabilities that match 5G, new requirements have been put forward for thermal conductivity solutions.

[0003] For high-power, high-density electronic devices, traditional silicone thermal pads alone cannot meet the temperature required for their normal operation.

[0004] Therefore, a thermally conductive pad with higher thermal conductivity is needed to meet this requirement.

[0005] Carbon fiber has excellent thermal conductivity, but the current method for preparing carbon fiber thermal conductive gaskets is single. Summary of the invention

[0006] The purpose of the embodiments of the present application is to provide a new method for preparing a carbon fiber thermally conductive gasket.

[0007] The present application provides a method for preparing a carbon fiber thermal conductive gasket, comprising:

[0008] Filling the mold cavity with a mixture of carbon fiber, adhesive and expansion agent; the volume of the mold cavity is variable, and the cavity is formed by an immovable first wall and a movable second wall; the second wall can be directional and movable along the X-axis;

[0009] The mold is baked so that the expansion agent in the mixture expands due to heat and generates shear force acting on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers in the mixture to be oriented.

[0010] Movable second wall Movable second wall Movable second wall Movable second wall The preparation method of the carbon fiber thermal conductive gasket provided in the present application is to fill a mixture of carbon fiber, adhesive and expansion agent into a mold cavity restricted in all directions, and bake it so that the expansion agent in the cavity expands due to heat. Since the second wall in the cavity can be directional moved along the X-axis, when the movable second wall expansion agent in the mixture is heated, a shear force is generated to act on the movable second wall, so that the movable second wall of the second wall moves in a directional manner along the X-axis, driving the carbon fibers to be directionally arranged, so that the disordered carbon fibers in the mixture form a directional arrangement.

[0011] Furthermore, the preparation method of the carbon fiber thermal conductive gasket of the present application has simple steps and only requires one baking of the mixture; it does not need to be baked multiple times. This is because the preparation method of the present application can vulcanize the mixture while baking the mixture in the mold, which reduces the preparation steps and improves efficiency.

[0012] The conventional method for preparing carbon fiber thermal conductive gaskets in the prior art requires that the carbon fibers be arranged in an oriented manner by electric field oriented arrangement, magnetic field oriented arrangement or extruder oriented arrangement, and then baked. After baking, a vulcanization step is performed. These preparation methods have more preparation steps and complicated processes. However, the preparation method of the present application can achieve oriented arrangement of carbon fibers and vulcanization at the same time with only one baking. Therefore, the preparation method of the present application has fewer process steps and is simpler.

[0013] In other embodiments of the present application, the expansion agent is selected from expandable microspheres, and the expandable microspheres, carbon fibers, and adhesive are uniformly mixed.

[0014] In other embodiments of the present application, the movable second wall includes a second wall body and an elastic member;

[0015] The elastic member is connected to the second wall body;

[0016] The expansion agent in the mixture expands under heat and generates shear force acting on the second wall body, so that the second wall body compresses the elastic member along the X-axis, and the elastic member generates reaction force acting on the second wall body.

[0017] In other embodiments of the present application, the elastic member is selected as a spring;

[0018] The spring includes a first spring and a second spring, and the second wall body includes a first body and a second body; the mold also includes a first limiter and a second limiter;

[0019] One end of the first spring is connected to the first limiter, and the other end is connected to the first body; one end of the second spring is connected to the second limiter, and the other end is connected to the second body;

[0020] The first body can move along the positive direction of the X-axis when the mixed material expands; the second body can move along the negative direction of the X-axis when the mixed material expands.

[0021] In other embodiments of the present application, baking the mold includes:

[0022] The mold is baked at 100°C-140°C.

[0023] In other embodiments of the present application, baking the mold includes:

[0024] Bake the mold for no less than 12 hours.

[0025] In other embodiments of the present application, the method includes:

[0026] After the mold cavity is filled with a mixture of carbon fiber, adhesive and expansion agent, vacuum is also performed to remove air from the mixture.

[0027] In other embodiments of the present application, the vacuuming time is 10 minutes to 30 minutes.

[0028] In other embodiments of the present application, the mold cavity is filled with a mixture of carbon fiber, adhesive and expansion agent, including:

[0029] After the mixture of carbon fiber, adhesive and expansion agent is filled into the mold cavity, the cavity is closed by a cover.

[0030] In other embodiments of the present application, the method further includes:

[0031] After the mold is baked, the formed green body is taken out and cut into sheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 A schematic diagram of the structure of the mold provided in the embodiment of the present application;

[0034] Figure 2 A schematic diagram of the structure of the mold cavity and cover body provided in the embodiment of the present application;

[0035] Figure 3 A schematic diagram of the structure of the cavity of the mold provided in an embodiment of the present application.

[0036] Icon: 100 - mold; 110 - cavity; 111 - first wall; 1112 - first side wall; 1113 - second side wall; 1114 - bottom wall; 120 - cover; 1301 - first body; 1302 - second body; 132 - first spring; 133 - second spring; 131 - first limiter; 134 - second limiter. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0038] Therefore, the following detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0039] Reference Figure 1-Figure 3 The present application provides a method for preparing a carbon fiber thermally conductive gasket, comprising:

[0040] Filling the mold cavity with a mixture of carbon fiber, adhesive and expansion agent; the volume of the mold cavity is variable, and the cavity is formed by an immovable first wall and a movable second wall; the second wall can be directional and movable along the X-axis;

[0041] The mold is baked so that the expansion agent in the mixture expands due to heat and generates shear force acting on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers in the mixture to be oriented.

[0042] Movable second wall Movable second wall Movable second wall Movable second wall The preparation method of the carbon fiber thermal conductive gasket provided in the present application, the preparation method of the carbon fiber thermal conductive gasket provided in the present application, by filling a mixture of carbon fiber, adhesive and expansion agent into a mold cavity restricted in all directions, and baking it, so that the expansion agent in the cavity expands due to heat. Since the second wall in the cavity can be directional and movable along the X-axis, when the expansion agent in the mixture is heated, a shear force is generated to act on the second wall, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers to be directionally arranged, so that the disordered carbon fibers in the mixture form a directional arrangement. Movable second wall Movable second wall Movable second wall While baking, the mixture can be cured and vulcanized at the same time, reducing the preparation steps and improving efficiency.

[0043] Furthermore, in some embodiments of the present application, a method for preparing a carbon fiber thermally conductive gasket comprises the following steps:

[0044] Step S1, preparing a mixture of carbon fiber, adhesive and expansion agent.

[0045] Further, in some embodiments of the present application, the preparation of the mixture of the above-mentioned carbon fiber, adhesive and expansion agent includes:

[0046] The carbon fiber, adhesive and expansion agent are mixed evenly according to a certain ratio.

[0047] In some embodiments of the present application, the step of uniformly mixing the carbon fiber, the adhesive and the expansion agent is to place the carbon fiber, the adhesive and the expansion agent in a centrifugal mixer and stir them uniformly.

[0048] Further optionally, the stirring time is 5-20 minutes. Exemplarily, the stirring time is 5 minutes, 8 minutes, 10 minutes, 15 minutes or 20 minutes.

[0049] Furthermore, in some embodiments of the present application, in the above-mentioned mixture, the adhesive includes vinyl silicone oil, silicone coupling agent, vulcanizing agent, catalyst and inhibitor.

[0050] The above-mentioned adhesive is baked, and the vinyl silicone oil undergoes a cross-linking reaction (also called a vulcanization reaction) under the conditions of a vulcanizer and a catalyst to form a network structure, thereby bonding the carbon fibers together.

[0051] Among them, coupling agents help powder filling;

[0052] The inhibitor slows down the reaction rate of vinyl silicone oil to avoid excessive reaction (sometimes it will vulcanize during stirring without adding an inhibitor), which will make subsequent processes unable to operate.

[0053] By adding inhibitors, the inhibitors evaporate slowly, making the vulcanization process proceed slowly.

[0054] Specifically, when the subsequent baking temperature reaches 100°C, the microspheres will expand (it may only take a few seconds to expand), but vulcanization is a slow process. The inhibitor will slowly evaporate first, and the material will slowly vulcanize from the outside to the inside, which generally takes several hours.

[0055] Furthermore, the inhibitor can also be volatilized through the high temperature of baking.

[0056] That is, the baking and vulcanization of the solution of the present application are carried out together.

[0057] Furthermore, in some embodiments of the present application, the above-mentioned selected silicone coupling agent, vulcanizing agent, catalyst and inhibitor can be selected from common commercial products in the field.

[0058] Further optionally, in some embodiments of the present application, the above-mentioned expansion agent is selected from expandable microspheres.

[0059] Further, the expanded microspheres, carbon fibers, and adhesive are uniformly mixed. For example, the weighed expanded microspheres, carbon fibers, vinyl silicone oil, silicone coupling agent, vulcanizing agent, catalyst, and inhibitor are placed in a centrifugal mixer and stirred for 10 minutes to uniformly mix the materials.

[0060] Expandable microspheres are thermoplastic hollow polymer microspheres, which consist of a thermoplastic polymer shell and an alkane gas sealed in. When the expanded microspheres are heated, the gas pressure in the shell increases and the thermoplastic shell softens, thereby significantly increasing the volume of the expanded microspheres.

[0061] It should be noted that the above-mentioned expanded microspheres can be selected from commercially available brands commonly used in the art.

[0062] Furthermore, in some embodiments of the present application, the above-mentioned mixed material also includes thermally conductive ceramic powder. The thermally conductive ceramic powder can be used as a thermally conductive powder filler.

[0063] Further optionally, the thermally conductive ceramic powder is selected from at least one of aluminum oxide and aluminum hydroxide.

[0064] Furthermore, in some embodiments of the present application, the ratio of the above-mentioned carbon fiber, thermal conductive ceramic powder, expanded microspheres, vinyl silicone oil, silicone coupling agent, vulcanizer, catalyst and inhibitor is: (50-110): (200-300): (2-10): (20-80): (0.5-1.5): (2.0-3.0): (1-3): (0.01-0.05).

[0065] Further optionally, in some embodiments of the present application, the ratio of the above-mentioned carbon fiber, thermal conductive ceramic powder, expanded microspheres, vinyl silicone oil, silicone coupling agent, vulcanizer, catalyst and inhibitor is: (60-100): (210-290) (3-8): (30-70): (0.6-1.4): (2.1-2.9): (1.5-2.5): (0.02-0.04).

[0066] Exemplarily, in some embodiments of the present application, the ratio of the above-mentioned carbon fiber, thermally conductive ceramic powder, expanded microspheres, vinyl silicone oil, silicone coupling agent, vulcanizer, catalyst and inhibitor is 60:270:5:50:0.7:2.5:2.0:0.03; or the ratio of the above-mentioned carbon fiber, thermally conductive ceramic powder, expanded microspheres, vinyl silicone oil, silicone coupling agent, vulcanizer, catalyst and inhibitor is 80:240:5:50:0.7:2.5:2.0:0.03; or the ratio of the above-mentioned carbon fiber, thermally conductive ceramic powder, expanded microspheres, vinyl silicone oil, silicone coupling agent, vulcanizer, catalyst and inhibitor is 100:300:5:50:0.7:2.5:2.0:0.03.

[0067] Furthermore, in some embodiments of the present application, the above-mentioned carbon fiber is selected from the asphalt-based carbon fiber commonly used in the art.

[0068] Asphalt-based carbon fiber itself has high thermal conductivity, and the thermal conductive pad made by directional arrangement of carbon fiber has good thermal conductivity and flexibility. The thermal conductivity coefficient in the fiber direction (length direction) can reach 600 W / m·K~1200W / m·K.

[0069] Step S2, filling the mold cavity with a mixture of carbon fiber, adhesive and expansion agent.

[0070] Furthermore, in some embodiments of the present application, the mold cavity is filled with a mixture of carbon fiber, adhesive and expansion agent, including:

[0071] After the mixture of carbon fiber, adhesive and expansion agent is filled into the mold cavity, the cavity is closed by a cover.

[0072] Furthermore, in some embodiments of the present application, after the mold cavity is filled with a mixture of carbon fiber, adhesive, and expansion agent, vacuuming is performed to remove air from the mixture.

[0073] By vacuuming, the pores in the final product can be greatly reduced, thus improving the product appearance quality.

[0074] Furthermore, in some embodiments of the present application, the volume of the cavity 110 of the mold 100 is variable, and the cavity 110 is formed by an immovable first wall 111 and a movable second wall; the second wall can be directional moved along the X-axis.

[0075] Further, refer to Figure 1 and Figure 2 In some embodiments of the present application, the mold 100 shown in the figure is used to fill the mixture obtained in step S1. The cover 120 is a part of the first wall 111 and cannot be moved after being closed, so as to limit the position of the mixture.

[0076] The mixed material obtained in step S1 is filled into the cavity 110 of the mold 100 , the air is exhausted, and then the cavity 110 is sealed.

[0077] Further, in some embodiments of the present application, exhausting air includes:

[0078] The mixed material in the cavity 110 is evacuated to discharge the air in the mixed material.

[0079] Furthermore, in some embodiments of the present application, the mixed material in the cavity 110 is evacuated for a period of 10 minutes to 30 minutes.

[0080] Further optionally, the mixed material in the cavity 110 is evacuated for a period of 11 minutes to 29 minutes.

[0081] Illustratively, the mixed material in the cavity 110 is evacuated for 12 minutes, 15 minutes, 18 minutes, 20 minutes, 22 minutes, 25 minutes, 26 minutes or 28 minutes.

[0082] By evacuating the mixture in the cavity 110, the air in the mixture can be completely sucked out, so that the mixture fills the cavity 110, so that the inner walls of the cavity 110 limit the mixture, and the expanded microspheres in the mixture can only expand in a preset direction, thereby driving the directional arrangement of the carbon fibers and achieving the effect of directional arrangement of the carbon fibers.

[0083] Furthermore, in some embodiments of the present application, a vacuum pump is used to evacuate the mixture. Specifically, the vacuum pump is placed in the mold cavity of the mold, and the mixture in the mold cavity is evacuated for 15 minutes to completely remove the air in the mixture.

[0084] Furthermore, in some embodiments of the present application, the mixture obtained in step S1 is filled into the cavity 110 of the mold 100, and after vacuuming, the cavity 110 is sealed with a cover 120. At this time, the mixture is restricted from displacement in all directions by the first wall 111 and the second wall of the cavity 110.

[0085] Further, in some embodiments of the present application, the movable second wall comprises a second wall body and an elastic member. The elastic member is connected to the second wall body. The expansion agent in the mixture expands under heat to generate a shear force acting on the second wall body, so that the second wall body compresses the elastic member along the X-axis, and the elastic member generates a reaction force acting on the second wall body.

[0086] Furthermore, in some embodiments of the present application, the elastic member is a spring.

[0087] Furthermore, in some embodiments of the present application, the spring includes a first spring 132 and a second spring 133 , the second wall body includes a first body 1301 and a second body 1302 ; the mold 100 also includes a first limiter 131 and a second limiter 134 .

[0088] Further, in some embodiments of the present application, one end of the first spring 132 is connected to the first stopper 131, and the other end is connected to the first body 1301; one end of the second spring 133 is connected to the second stopper 134, and the other end is connected to the second body 1302. The first body 1301 can move along the positive direction of the X axis when the mixture expands; the second body 1302 can move along the negative direction of the X axis when the mixture expands.

[0089] Further, refer to Figure 1 and Figure 2In some embodiments of the present application, the cover 120 is covered with the first stopper 131 and the second stopper 134. The first stopper 131 and the second stopper 134 are connected to the first wall 111 of the mold 100.

[0090] Reference Figure 1-Figure 3 In the illustrated embodiment, the mold 100 is in the shape of a cuboid. The cavity 110 is in the shape of a cuboid. The first wall 111 of the cavity 110 includes a first side wall 1112, a second side wall 1113, a bottom wall 1114, and a cover 120. The first side wall 1112, the second side wall 1113, the bottom wall 1114, the cover 120, the first body 1301, and the second body 1302 enclose the cavity 110. The first side wall 1112, the second side wall 1113, and the bottom wall 1114 extend outwardly and are connected to the first limit piece 131 and the second limit piece 134 to form an integral mold 100, so that there is a space between the first limit piece 131 and the second limit piece 134, and the aforementioned first spring 132 and second spring 133 are accommodated in the space here, one end of the first spring 132 is connected to the first body 1301, and the other end is connected to the second side wall 1113; one end of the first spring 132 is connected to the first body 1301, and the other end is connected to the first limit piece 131; one end of the second spring 133 is connected to the second body 1302, and the other end is connected to the second limit piece 134, and can generate elastic force on the first body 1301 and the second body 1302.

[0091] Reference Figure 1 When the mixture of carbon fiber, adhesive and expansion agent is filled into the cavity 110 of the mold 100 and the cavity 110 is closed by the cover 120, the wall of the cavity 110 and the cover 120 limit the mixture in the cavity 110 from different directions, and only the second wall in the cavity can move away from each other along the X-axis after being subjected to force.

[0092] In other optional embodiments of the present application, the above-mentioned movable second wall may be provided with only one, for example, movable only along the positive direction of the X-axis; or movable only along the negative direction of the X-axis.

[0093] The mold is provided with a spring, which can generate elastic force during the baking process, so that the material at the end of the product is compactly formed, so that the shape is better when cut into sheets, and the utilization rate of the raw materials is improved.

[0094] In other optional embodiments of the present application, the shape of the above-mentioned cavity can also be set to other shapes.

[0095] Step S3, baking the mold so that the expansion agent in the mixture expands due to heat and generates shear force acting on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers in the mixture to be oriented.

[0096] The mold filled with the mixture in step S2 is baked. During this process, the expansion agent in the mixture in the mold cavity expands due to heat and acts on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers in the mixture to be oriented.

[0097] The conventional method for preparing carbon fiber thermal conductive gaskets in the prior art requires that the carbon fibers be arranged in an oriented manner by electric field oriented arrangement, magnetic field oriented arrangement or extruder oriented arrangement, and then baked. After baking, a vulcanization step is performed. These preparation methods have more preparation steps and complicated processes. However, the preparation method of the present application can achieve oriented arrangement of carbon fibers and vulcanization at the same time with only one baking. Therefore, the preparation method of the present application has fewer process steps and is simpler.

[0098] Furthermore, in some embodiments of the present application, the expanded microspheres in the mixture expand due to heat after baking, generating a shear force acting on the movable second wall, so that the movable second wall moves along the X-axis, driving the carbon fibers to be oriented.

[0099] Reference Figure 1 In the illustrated embodiment, when the closed mold is baked, the shear force generated by the expansion of the expanded microspheres acts on the first body and the second body, and the first body and the second body compress the elastic member along the positive direction of the X-axis and the negative direction of the X-axis respectively, driving the carbon fibers to be oriented along the positive direction of the X-axis and the negative direction of the X-axis.

[0100] It should be noted that in the art, the directional arrangement of carbon fibers is a concept of rough orientation, and a certain deviation is allowed. For example, the directional arrangement along the X-axis direction of the carbon fibers mentioned above is not absolutely along the X-axis. Some carbon fibers may be directional along the X-axis direction, and some carbon fibers may have a certain angle with the X-axis, which are all allowed in the art and fall within the error range known in the art.

[0101] Further, in some embodiments of the present application, baking the mold includes:

[0102] The mold is baked at 100°C-140°C.

[0103] Further optionally, in some embodiments of the present application, baking the mold comprises:

[0104] The mold is baked at 101°C-139°C.

[0105] For example, in some embodiments of the present application, baking the mold includes:

[0106] The mold is baked at 105°C, 108°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C.

[0107] By baking the mold within the above temperature range, the silicone coupling reaction and vulcanization can be achieved simultaneously, saving steps and improving production efficiency.

[0108] Further, in some embodiments of the present application, baking the mold includes:

[0109] Bake the mold for no less than 12 hours.

[0110] Further optionally, in some embodiments of the present application, baking the mold comprises:

[0111] The mold is baked for 12 hours to 48 hours.

[0112] Further optionally, in some embodiments of the present application, baking the mold comprises:

[0113] The mold is baked for 12 hours to 36 hours.

[0114] For example, in some embodiments of the present application, baking the mold includes:

[0115] The mold is baked for 12h, 13h, 15h, 20h, 24h, 26h, 30h, 34h or 40h.

[0116] By baking the mold within the above-mentioned range, the baking effect can be ensured.

[0117] The silicone coupling agent in the mixture undergoes a coupling reaction with the vinyl silicone oil, and is vulcanized simultaneously during the baking process under the action of the vulcanizing agent to form a solid green body.

[0118] Step S4: After baking the mold, take out the formed blank, and cut the blank into sheets along the direction of the directional arrangement of the carbon fibers.

[0119] In some embodiments of the present application, the solid blank obtained in step S3 is taken out from the mold cavity, and then the blank is cut into sheets of a certain thickness along the direction of the directional arrangement of the carbon fibers according to actual needs, and the sheets can be used as thermal conductive pads.

[0120] Exemplarily, in the illustrated embodiment, the carbon fibers are arranged in a direction along the x-axis (i.e., the length direction of the cavity in the figure). When the solid blank is taken out of the mold cavity, the blank is cut into sheets of a certain thickness along the length direction of the blank. At this time, the cutting is done along the direction of the directional arrangement of the carbon fibers. Therefore, the carbon fibers in each sheet obtained are arranged in a direction. The carbon fibers are arranged in a direction along the thickness direction of the gasket, that is, the carbon fibers are vertically distributed in the thickness direction of the gasket.

[0121] It should be noted that in the embodiments of the present application, the length of the carbon fiber used is 100 μm-200 μm. Further optionally, in the embodiments of the present application, the length of the carbon fiber used is 105 μm-195 μm. Exemplarily, in some embodiments of the present application, the length of the above-mentioned carbon fiber is 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm or 190 μm.

[0122] Further, in some embodiments of the present application, the solid blank obtained in step S3 is taken out from the mold cavity and then cut into sheets of a certain thickness according to actual needs, and the thickness of the sheet is selected from 1 mm to 3 mm. For example, the thickness of the sheet is selected from 1.5 mm, 2 mm, 2.5 mm or 3 mm.

[0123] Since the thickness of the cut sheet is much greater than the length of the carbon fiber, the carbon fiber in the single layer will hardly be affected during the cutting process, so it can be ensured that multiple directional carbon fibers are distributed in the single-layer gasket obtained by cutting. The carbon fiber has anisotropic thermal conductivity, and the thermal conductivity coefficient in the fiber direction (length direction) can reach 600 W / m·K~1200W / m·K. This can improve the thermal conductivity of the thermally conductive gasket.

[0124] The features and performance of the present application are further described in detail below in conjunction with the embodiments:

[0125] Example 1

[0126] A carbon fiber thermal conductive pad is provided, which is prepared according to the following steps:

[0127] S1. Prepare a mixture.

[0128] Prepare the following raw materials:

[0129] Carbon fiber with a length of 150 μm was purchased from the brand agent of Mitsubishi Chemical in Japan;

[0130] Lightweight alumina with a particle size of 1 μm-5 μm was purchased from the Letu brand agent;

[0131] Spherical alumina with a particle size of 5 μm-10 μm was purchased from Foshan Sanshui Jinge brand;

[0132] Vinyl silicone oil, purchased from Shin-Etsu brand agent;

[0133] Expandable microspheres 120DU15 were purchased from the SFEP brand import agent;

[0134] Silicone coupling agent KBM903; purchased from Shin-Etsu brand agent;

[0135] Platinum curing agent was purchased from Dongguan Dongsheng Synthetic Materials Co., Ltd.

[0136] Platinum catalyst was purchased from Dongguan Dongsheng Synthetic Materials Co., Ltd.

[0137] Inhibitor methylbutynol.

[0138] After weighing the various raw materials according to the proportions in Table 1, put them into a centrifugal mixer and stir for 10 minutes to mix the various raw materials evenly.

[0139] Step S2: Place the raw materials mixed evenly in step S1 into Figure 1 In the mold cavity shown, use a vacuum pump to evacuate the air in the mixture for 15 minutes, then cover the mold with a cover plate and tighten the screws.

[0140] Step S3, putting the mold closed in step S2 into a 100°C oven and baking for 12 hours. Through the outward expansion force of the expanded microspheres and the limitation of the four walls of the mold, the shear force generated by the directional expansion of the expanded microspheres drives the carbon fibers to align in a directional manner, thereby achieving the purpose of orientation.

[0141] Step S4, take out the mold baked in step S3 from the oven, let it stand for 10 minutes, then unscrew the screws, take out the formed embryo, and cut it into multiple rectangular sheets along the length direction of the rectangular embryo. The thickness of the sheet sample is 2mm, and the length and width of the sheet sample are both 25mm.

[0142] Example 2

[0143] A carbon fiber thermal conductive gasket is provided, and its preparation steps are the same as those in Example 1, except that the ratio of the mixture in step 1 is different, as shown in Table 1.

[0144] Example 3

[0145] A carbon fiber thermal conductive gasket is provided, and its preparation steps are the same as those in Example 1, except that the ratio of the mixture in step 1 is different, as shown in Table 1.

[0146] Example 4

[0147] A carbon fiber thermal conductive gasket is provided, and its preparation steps are the same as those in Example 1, except that the test thickness is different, as shown in Table 1.

[0148] Example 5

[0149] A carbon fiber thermal conductive gasket is provided, and the preparation steps are the same as those of Example 1, except that when the mold of Example 1 is used, the spring is removed.

[0150] Example 6

[0151] A carbon fiber thermally conductive gasket is provided, and the preparation steps are the same as those in Example 1, except that vacuuming is not performed before baking.

[0152] Table 1

[0153]

[0154]

[0155] Comparative Example 1

[0156] A thermally conductive gasket is provided, and the preparation steps thereof are the same as those of Example 1, except that there is no carbon fiber in the raw material of step S1.

[0157] Comparative Example 2

[0158] A thermally conductive gasket is provided, and the preparation steps thereof are the same as those of Example 1, except that there are no expanded microspheres in the raw materials of step S1.

[0159] Experimental Example 1

[0160] The performance of the carbon fiber thermal conductive gaskets prepared in Examples 1-6 and Comparative Examples 1-2 was tested.

[0161] (1) Thermal conductivity

[0162] Detection method: Use Ruiling Thermal Tester (Model LW-9389) for detection.

[0163] (2) Thermal resistance

[0164] Test method: Use Ruiling Thermal Tester (Model LW-9389) for testing. The test results are shown in Table 2.

[0165] Table 2

[0166]

[0167] From the results in Table 2 above, it can be seen that the carbon fiber thermal conductive pads prepared in various embodiments provided in the present application have a thermal conductivity of 19.55 W / m·K to 25.01 W / m·K when the thickness is 2 mm, and a thermal resistance of 0.653°C cm2 / w~0.923℃cm 2 / w.

[0168] However, the thermal conductivity of the thermally conductive gaskets provided in Comparative Examples 1 and 2 is only 2.83 to 3.16 W / m·K, which is significantly lower than the thermal conductivity of the carbon fiber thermally conductive gasket in the embodiment of the present application.

[0169] The thermal resistance of the thermally conductive pads provided in Comparative Examples 1 and 2 is 5.657°C cm 2 / w~7.005℃cm 2 / w, which is significantly higher than the thermal resistance of the carbon fiber thermal conductive gasket in the embodiment of the present application.

[0170] It can be seen that the thermal conductivity of the thermally conductive gaskets of Comparative Examples 1 and 2 is lower than that of the present application.

[0171] This indicates that the carbon fiber thermal conductive gasket prepared in the embodiment of the present application has excellent thermal conductivity.

[0172] Furthermore, the thermally conductive gaskets provided in Examples 5 and 6 also have better thermal conductivity and thermal resistance.

[0173] The main difference between Example 5 and Example 1 is the appearance of the product. The material at the end of the product of Example 5 is loose and easily breaks when cut into sheets, which reduces the utilization rate of the raw materials.

[0174] The main difference between Example 6 and Example 1 lies in the product appearance. There are pores in the product of Example 6, and when the product is cut into sheets, there will be holes, which affects the product appearance.

[0175] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a carbon fiber thermal conductive pad, characterized in that: include: Filling the mold cavity with a mixture of carbon fiber, adhesive and expansion agent; The volume of the cavity of the mold is variable, and the cavity is formed by an immovable first wall and a movable second wall; the second wall can be directional and movable along the X-axis; The mold is baked so that the expansion agent in the mixture expands due to heat and generates a shear force acting on the second wall, and the second wall generates a reverse resisting force acting on the mixture; the shear force is greater than the resisting force, so that the second wall moves in a directional manner along the X-axis, driving the carbon fibers in the mixture to be oriented; the movable second wall comprises a second wall body and an elastic member; The elastic member is connected to the second wall body; The expansion agent in the mixture expands when heated and generates a shear force acting on the second wall body, so that the second wall body compresses the elastic member along the X-axis, and the elastic member generates a reaction force acting on the second wall body.

2. The method for preparing the carbon fiber thermal conductive pad according to claim 1, characterized in that: The expansion agent is selected from expansion microspheres, and the expansion microspheres, the carbon fibers and the adhesive are uniformly mixed.

3. The method for preparing the carbon fiber thermal conductive pad according to claim 1, characterized in that: The elastic member is selected as a spring; The spring includes a first spring and a second spring, and the second wall body includes a first body and a second body; the mold also includes a first limiter and a second limiter; One end of the first spring is connected to the first limiter, and the other end is connected to the first body; one end of the second spring is connected to the second limiter, and the other end is connected to the second body; The first body can move along the positive direction of the X-axis when the mixed material expands; the second body can move along the negative direction of the X-axis when the mixed material expands.

4. The method for preparing a carbon fiber thermally conductive gasket according to any one of claims 1 to 3, characterized in that: The step of baking the mold comprises: The mold is baked at 100°C-140°C.

5. The method for preparing the carbon fiber thermal conductive pad according to claim 4, characterized in that: The step of baking the mold comprises: The mold is baked for no less than 12 hours.

6. The method for preparing the carbon fiber thermal conductive pad according to claim 4, characterized in that: The method comprises: After the mold cavity is filled with a mixture of carbon fiber, adhesive and expansion agent, vacuum is also performed to remove air in the mixture.

7. The method for preparing a carbon fiber thermally conductive gasket according to claim 6, characterized in that: The vacuuming time is 10 minutes to 30 minutes.

8. The method for preparing a carbon fiber thermally conductive gasket according to claim 1, characterized in that: Fill the mold cavity with a mixture of carbon fiber, adhesive and expansion agent, including: After the mixture of the carbon fiber, the adhesive and the expansion agent is filled into the mold cavity, the cavity is closed by using a cover.

9. The method for preparing a carbon fiber thermally conductive gasket according to claim 1, characterized in that: The method further comprises: After the mold is baked, the formed green body is taken out and cut into sheets along the direction of the directional arrangement of the carbon fibers.

Citation Information

Patent Citations

  • Process for the production of composite molded articles

    CA2020956A1

  • Preparation method of carbon-based composite material with high heat conductivity coefficients in both plane direction and thickness direction

    CN104446587A

  • Method for molding resin fiber composite from spontaneous thermal-expansion pressure bag

    CN104647674A

  • Heat-conductive foam cotton with heat conductivity

    CN109608865A

  • Molded body

    CN1953828A