Catalyst and preparation method thereof and method for synthesizing isoprene
By loading catalysts with metal oxides such as TiO2, Pd, Zr, Gd on SiO2 or γ-Al2O3 support, the problems of low raw material selectivity and environmental pollution in isoprene synthesis are solved, and efficient and environmentally friendly isoprene is achieved. Diene synthesis extends the catalyst life and meets the needs of industrial production.
Patent Information
- Application Number
- CN202310399586.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-14
AI Technical Summary
The existing isoprene synthesis methods have problems such as low raw material selectivity, serious equipment corrosion, difficulty in separation of products and catalysts, and serious environmental pollution. Especially the preparation process of traditional supported catalysts has a large environmental pollution and short catalytic life, which is limited. Its industrial application.
Using catalysts including transition metal oxides such as TiO2, Pd, Zr, Gd, etc., to form solid bonds through support such as SiO2 or γ-Al2O3, to regulate metal dispersion forms, reduce acid content, improve catalytic performance and conversion rate, the preparation method is simple, Non-toxic, suitable for industrial production.
It has achieved high formaldehyde conversion, isobutene selectivity and isoprene yield, extended catalyst life, meets industrial production needs, and conforms to the concept of green and environmental protection.
Smart Images

Figure HDA0004178934740000011 
Figure HDA0004178934740000012
Abstract
Description
Technical Field
[0001] The invention relates to the field of diene synthesis, in particular to a catalyst and a preparation method thereof and a method for synthesizing isoprene. Background Art
[0002] Isoprene (C 5 H 8 ) is a monomer of many artificial synthetic rubbers, among which cis-1,4-polyisoprene rubber is one of the best-performing synthetic rubbers, which can replace natural rubber and is also a raw material for synthesizing vitamins, carotene, pesticides, spices, lubricants, vulcanizers, etc. It can be seen that isoprene has a significant impact on people's daily life and social development. With the progress of the times, the demand for isoprene is increasing day by day. The output of isoprene in the C5 fraction resources alone cannot meet our needs. The development of new synthetic isoprene routes has become a hot topic of social concern. At present, the main method for producing isoprene is the two-step method, but this method has problems such as low raw material selectivity, serious corrosion to equipment, difficulty in separating products and catalysts, and serious environmental pollution. The gas phase one-step method is a multiphase reaction, which is easy to separate. At the same time, it has the advantages of low equipment requirements, simple operation, short process flow, and can improve the selectivity of raw materials, so it has been paid attention to and studied by a large number of scientific researchers.
[0003] The gas phase one-step method mainly uses heterogeneous catalysts for the reaction, which include metal oxide catalysts, supported catalysts, molecular sieve catalysts, etc. At present, the traditional supported catalyst is Cr-P / SiO 2 , but it is toxic, pollutes the environment, has high preparation cost and short catalytic life. Xu Shan et al. disclosed a supported acid-base bifunctional catalyst, with formaldehyde selectivity of up to 90.7% and conversion rate of up to 85.3%. The catalyst is characterized by achieving the result of catalyst acid-base synergy by loading alkali metal elements and washing with ammonia water, but a large amount of ammonia water is required to wash the catalyst intermediate in the preparation process, which pollutes the environment and is not conducive to industrial production (CNIO6563459A). It can be seen from this that although supported catalysts have advantages such as simple preparation and low cost compared to most catalysts, their preparation process may pollute the environment, which limits its application in industry, and it is urgent to develop environmentally friendly catalysts with good catalytic performance.
[0004] In addition, although it can be introduced into carriers such as SiO 2 Improve the catalytic performance of the catalyst, but the presence of transition metal elements in SiO 2 The risk of uncontrolled surface dispersion forms limits the low-cost, pollution-free SiO 2 Application in the field of enal condensation. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a catalyst and a preparation method thereof and a method for synthesizing isoprene. The catalyst provided by the present invention is used for synthesizing isoprene and has high formaldehyde conversion rate, isobutylene selectivity and isoprene yield.
[0006] The present invention provides a catalyst, which comprises a carrier and a first transition metal oxide, a second transition metal oxide and a rare earth metal oxide loaded on the carrier;
[0007] The first transition metal and the second transition metal are different;
[0008] The first transition metal oxide is TiO 2 .
[0009] The catalyst of the present invention comprises a carrier, wherein the carrier is selected from SiO 2 ,γ-Al 2 O 3 , MgO, CaO, MnO or BaO, preferably selected from SiO 2 or γ-Al 2 O 3 .
[0010] The catalyst of the present invention comprises a first transition metal oxide supported on the carrier, wherein the first transition metal oxide is TiO 2 .TiO 2 It forms a strong bond with the surface of the carrier, reduces the loss of metal elements during the reaction, and prolongs the life of the catalyst; TiO 2 The dispersion form of transition metal oxides on its surface can be flexibly adjusted; TiO 2 The acid content and total acid content of the rare earth metal oxide in the catalyst are appropriately reduced, the occurrence of side reactions is reduced, and the conversion rate of the raw materials is improved. In certain embodiments of the present invention, the loading amount of the first transition metal is 5% to 50%, preferably 10% to 20%.
[0011] The catalyst of the present invention further comprises a second transition metal oxide and a rare earth metal oxide supported on the carrier. The second transition metal of the present invention is selected from Pd, Zr, Cs, Mo, V, Cu, Zn, Cr, Fe, Co or Ni, preferably selected from one of Pd, Cs, Mo, V, Cu or Zr, and most preferably selected from Zr; the rare earth metal oxide is selected from La, Ce, Rb, Pr, Gd, Er, Tm, Sm, Tb or Ho, preferably selected from one of La, Ce or Gd, more preferably selected from Ce or Gd, and most preferably selected from Gd. In certain embodiments of the present invention, the loading amount of the second transition metal oxide is 0.1% to 10%, preferably 1% to 2%; the loading amount of the rare earth metal oxide is 0.1% to 10%, preferably 1% to 2%.
[0012] The present invention provides a method for preparing the above catalyst, comprising the following steps:
[0013] Step 1) mixing a titanium source solution and a carrier, and performing a first calcination;
[0014] Step 2) Mixing a second transition metal source, a rare earth metal source and the product obtained in step 1), and performing a second calcination to obtain the catalyst.
[0015] The present invention first prepares a titanium source solution. Specifically, the present invention mixes a titanium source and an organic solvent, and adjusts the pH to acidic to obtain a titanium source solution. In certain embodiments of the present invention, the present invention mixes a titanium source and an organic solvent, and adds a mixed solution of an organic acid and the organic solution thereto to adjust the pH to acidic to obtain a titanium source solution.
[0016] The titanium source of the present invention is selected from at least one of tetrabutyl titanate, dibutyl titanate or diethyl titanate; the organic solvent is selected from at least one of ethanol, methanol, isopropanol or ethylene glycol; the organic acid is selected from at least one of glacial acetic acid, salicylic acid, citric acid, 5-sulfosalicylic acid, malic acid or oxalic acid, preferably at least one of glacial acetic acid, 5-sulfosalicylic acid or oxalic acid. The volume ratio of the titanium source of the present invention to the organic solvent is 1: (1 to 50), preferably 1: (10 to 15). The concentration of the organic acid of the present invention is 0.01 mol / L to 2 mol / L, preferably 0.01 mol / L.
[0017] The pH value will affect the crystal form and particle size of the first calcined product of the titanium source solution. The pH value of the titanium source solution of the present invention is 1 to 6, preferably 1.3 to 4.8. In one embodiment, under magnetic stirring, tetrabutyl titanate is slowly dripped into anhydrous ethanol to mix to obtain a uniform light yellow solution, and then the mixed solution of the organic acid and the organic solution is slowly dripped into the light yellow solution under stirring to adjust the pH value of the solution to obtain a titanium source solution.
[0018] After the titanium source solution is prepared in the present invention, the titanium source solution and the carrier are treated by an equal volume impregnation method. Specifically, after the titanium source solution is prepared in the present invention, the titanium source solution and the carrier are mixed and a first calcination is performed. In certain embodiments of the present invention, the carrier is immersed in the titanium source solution and allowed to stand at room temperature, dried, first calcined, and ground to obtain a carrier with nano-TiO 2 The carrier. The carrier needs to be treated with neutral deionized water before use to remove surface impurities. In one embodiment, the present invention immerses the carrier in the titanium source solution and leaves it to stand at room temperature for 24 hours, and then dries it at 120°C for 12 hours to perform a first calcination. The temperature of the first calcination of the present invention is 300°C to 1000°C, and the time of the first calcination is 2h to 8h; the temperature of the first calcination is preferably 500°C to 700°C, and the time of the first calcination is preferably 5h. After the first calcination, the loading amount of the product of the titanium source solution in the carrier is 5% to 50%, preferably 10% to 20%.
[0019] The carrier of the present invention needs to be cleaned before step 1). Specifically, the carrier is soaked in boiling water and then calcined to obtain a cleaned carrier. In certain embodiments of the present invention, the carrier is boiled in neutral deionized water for 1 hour, rinsed with cold deionized water 3 times, dried at 120°C, and calcined at 500°C for 5 hours to obtain a cleaned carrier.
[0020] After the first calcination, the present invention mixes the second transition metal source, the rare earth metal source and the product obtained in the above step 1) and performs a second calcination to obtain the catalyst of the present invention. The present invention mixes the second transition metal source, the rare earth metal source and the product obtained in the above step 1) by an equal volume impregnation method; specifically, the present invention drops an aqueous solution of the second transition metal source and the rare earth metal source into the product obtained in the above step 1), leaves it to stand at room temperature, dries it, and performs a second calcination to obtain the catalyst of the present invention. In certain embodiments of the present invention, the present invention dissolves the second transition metal source in water, ultrasonically disperses it for 5 minutes, obtains an aqueous solution of the second transition metal, dissolves the rare earth metal source in the aqueous solution of the second transition metal, ultrasonically disperses it for 5 minutes, obtains an aqueous solution of the second transition metal source and the rare earth metal source; drops the aqueous solution of the second transition metal source and the rare earth metal source into the product obtained in the above step 1), leaves it to stand at room temperature, dries it, performs a second calcination, and grinds it into powder to obtain the catalyst of the present invention.
[0021] The second transition metal source of the present invention is selected from at least one of soluble salts such as vanadium tetrachloride, zinc nitrate, chromium nitrate hexahydrate, ferric chloride, cobalt carbonate, nickel nitrate, zirconium oxynitrate, palladium chloride, palladium nitrate, cesium carbonate, ammonium molybdate tetrahydrate, and copper nitrate; the rare earth metal source is selected from at least one of soluble salts such as lanthanum nitrate, cerium chloride, ammonium cerium nitrate, gadolinium nitrate, antimony chloride, praseodymium sulfate, erbium chloride, thulium nitrate, terbium chloride, and holmium trichloride.
[0022] The temperature of the second calcination of the present invention is 300℃~1000℃, and the time of the second calcination is 2h~8h; the temperature of the second calcination is preferably 500℃~700℃, and the time of the second calcination is preferably 5h. After the second calcination, the loading amount of the product of the second transition metal source in the above-mentioned carrier is 0.1%~10%, preferably 1%~2%; after the second calcination, the loading amount of the product of the rare earth metal source in the above-mentioned carrier is 0.1%~10%, preferably 1%~2%. The preparation method of the catalyst provided by the present invention is simple in process, and the raw materials are cheap, easy to obtain and non-toxic, which can meet the needs of industrial production and conform to the concept of green environmental protection.
[0023] The present invention also provides a method for synthesizing isoprene, comprising the following steps:
[0024] Under the action of the above catalyst, formaldehyde and isobutylene are reacted to obtain isoprene.
[0025] The present invention adopts a gas phase one-step method to synthesize isoprene, and the gas phase one-step method has the advantages of short reaction process, lower equipment requirements than the liquid phase method, and low cost. In certain embodiments of the present invention, the present invention uses formaldehyde and isobutylene as raw materials and nitrogen as a carrier under the action of the above-mentioned catalyst, and performs a Prins reaction in a fixed bed reactor at high temperature and normal pressure to obtain isoprene. The filling amount of the catalyst of the present invention is 0.5mL~5mL. Before the reaction, the catalyst is treated in a nitrogen atmosphere at 200℃~600℃ and 50mL / min for 2h~5h to remove impurities retained in the system and ensure that the reactants and products can pass through the reaction system smoothly.
[0026] The mass ratio of formaldehyde, isobutylene and catalyst used in the present invention is (0.05-0.5): (50-150): (0.5-5). In one embodiment, the feed rate of formaldehyde is 0.05 mL / min-0.5 mL / min; the feed rate of isobutylene is 50 mL / min-150 mL / min; the flow rate of nitrogen is 10 mL / min-60 mL / min. In one embodiment, the reaction temperature is 200°C-600°C.
[0027] The present invention provides a catalyst, which comprises a carrier and a first transition metal oxide, a second transition metal oxide and a rare earth metal oxide loaded on the carrier; the first transition metal and the second transition metal are different; the first transition metal oxide is TiO 2 The catalyst provided by the present invention has high formaldehyde conversion rate, isobutylene selectivity and isoprene yield for synthesizing isoprene. Experiments show that the formaldehyde conversion rate, isobutylene selectivity and isoprene yield of the catalyst provided by the present invention are much higher than those of the comparative example, wherein Zr-Gd / TiO 2 -SiO 2 The catalyst has a formaldehyde conversion rate of up to 95%, an isobutylene selectivity of up to 76%, and an isoprene yield of up to 50%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The catalyst provided by the present invention is SiO 2 Preparation flow chart when it is a carrier;
[0029] Figure 2 Schematic diagram of the apparatus for synthesizing isoprene. DETAILED DESCRIPTION
[0030] The present invention discloses a catalyst and a method for preparing the same, and a method for synthesizing isoprene. A person skilled in the art may refer to the contents of this invention and appropriately improve the process parameters to achieve the above. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this invention without departing from the content, spirit and scope of the present invention to achieve and apply the technology of the present invention.
[0031] The preparation steps of the catalyst provided by the present invention are as follows Figure 1 As shown, Figure 1 The catalyst provided by the present invention is SiO 2 The present invention prepares isoprene by using the provided catalyst, such as Figure 2 As shown, Figure 2 Schematic diagram of the apparatus for synthesizing isoprene.
[0032] The present invention will be further described below in conjunction with embodiments:
[0033] Example 1
[0034] 5 mL of tetrabutyl titanate was measured and slowly added to 5 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 2. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drip onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0035] Weigh 1.89 g zirconium oxynitrate and dissolve it in 10 mL deionized water, and disperse it ultrasonically for 5 min to obtain a clear zirconium oxynitrate solution. Then weigh 0.2 g gadolinium nitrate nonahydrate and dissolve it in the zirconium nitrate solution, and disperse it ultrasonically for 5 min to obtain a clear Zr-Gd mixed solution. The mixed solution was dropped into 10 g TiO 2 -C carrier surface, standing at room temperature for 24h, drying at 120℃ for 12h, and calcining at 500℃ for 5h to obtain Zr-Gd / TiO 2 -C catalyst, in which ZrO 2 The loading amount is 1%, Gd 2 O 3 The loading was 1%.
[0036] Weigh 3.0 mL Zr-Gd / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 92%, the isobutylene selectivity was 73%, and the isoprene yield was 45%.
[0037] Example 2
[0038] 5 mL of tetrabutyl titanate was measured and slowly added to 7.5 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 4. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drop the mixture onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0039] Weigh 1.89 g zirconium oxynitrate and dissolve it in 10 mL deionized water, and disperse it ultrasonically for 5 min to obtain a clear zirconium oxynitrate solution. Then weigh 0.2 g gadolinium nitrate nonahydrate and dissolve it in the zirconium nitrate solution, and disperse it ultrasonically for 5 min to obtain a clear Zr-Gd mixed solution. The mixed solution was dropped into 10 g TiO 2 -SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Zr-Gd / TiO 2 -SiO 2 Catalyst, ZrO 2 The loading amount is 1%, Gd 2 O 3 The loading was 1%.
[0040] Weigh 3.0 mL Zr-Gd / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 95%, the isobutylene selectivity was 76%, and the isoprene yield was 50%.
[0041] Example 3
[0042] 5 mL of tetrabutyl titanate was measured and slowly added to 7.5 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 4. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drop the mixture onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0043] Weigh 0.3 g of palladium chloride and dissolve it in 10 mL of deionized water. Ultrasonic dispersion is performed for 5 min to obtain a clear palladium chloride solution. Then, weigh 0.2 g of gadolinium nitrate nonahydrate and dissolve it in the palladium chloride solution. Ultrasonic dispersion is performed for 5 min to obtain a clear Pd-Gd mixed solution. The mixed solution is dropped into 10 g of TiO 2 -SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Pd-Gd / TiO 2 -SiO 2 The catalyst contains 1.2% PdO and 1.2% Gd 2 O 3 The loading was 1%.
[0044] Weigh 3.0 mL Pd-Gd / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 85%, the isobutylene selectivity was 70%, and the isoprene yield was 36%.
[0045] Example 4
[0046] 5 mL of tetrabutyl titanate was measured and slowly added to 10 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 4. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drip onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0047] Weigh 0.3 g of palladium chloride and dissolve it in 10 mL of deionized water. Ultrasonic dispersion is performed for 5 min to obtain a clear palladium chloride solution. Then, weigh 0.3 g of ammonium cerium nitrate and dissolve it in the palladium chloride solution. Ultrasonic dispersion is performed for 5 min to obtain a clear Pd-Ce mixed solution. The mixed solution is dropped into 10 g of TiO 2 -SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Pd-Ce / TiO 2 -SiO 2 The catalyst contains 1.2% PdO and 1.2% CeO 2 The loading was 1%.
[0048] Weigh 3.0 mL Pd-Ce / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 89%, the isobutylene selectivity was 77%, and the isoprene yield was 40%.
[0049] Comparative Example 1
[0050] Prepare a 0.01 mol / L acetic acid-anhydrous ethanol mixed solution, in which anhydrous ethanol is the solvent and acetic acid is the solute. Take 14 mL of this solution and drip it onto 10 g of clean nano-SiO using an equal volume immersion method. 2 The surface was allowed to stand at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain the acid-treated C carrier.
[0051] Weigh 0.3 g of palladium chloride and dissolve it in 10 mL of deionized water, and disperse it ultrasonically for 5 min to obtain a clear palladium chloride solution. Then weigh 0.3 g of ammonium cerium nitrate and dissolve it in the palladium chloride solution, and disperse it ultrasonically for 5 min to obtain a clear Pd-Ce mixed solution. The mixed solution was dropped into 10 g of SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Pd-Ce / SiO 2 The catalyst contains 1.2% PdO and 1.2% CeO 2 The loading was 1%.
[0052] Weigh 3.0 mL Pd-Ce / SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 80%, the isobutylene selectivity was 65%, and the isoprene yield was 35%.
[0053] Comparative Example 2
[0054] 5 mL of tetrabutyl titanate was measured and slowly added to 5 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 2. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drip onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0055] Weigh 0.3 g of niobium oxalate and dissolve it in 10 mL of deionized water, and disperse it ultrasonically for 5 min to obtain a clear niobium oxalate solution. Then weigh 0.2 g of gadolinium nitrate nonahydrate and dissolve it in the niobium oxalate solution, and disperse it ultrasonically for 5 min to obtain a clear Nb-Gd mixed solution. The mixed solution was dropped into 10 g of TiO by equal volume impregnation method. 2 -SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Nb-Gd / TiO2 -SiO 2 Catalyst, Nb 2 O 5 The loading amount is 1%, Gd 2 O 3 The loading was 1%.
[0056] Weigh 3.0 mL Nb-Gd / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 90%, the isobutylene selectivity was 70%, and the isoprene yield was 43%.
[0057] Comparative Example 3
[0058] 5 mL of tetrabutyl titanate was measured and slowly added to 7.5 mL of anhydrous ethanol under magnetic stirring to obtain a uniform light yellow tetrabutyl titanate solution. Next, a 0.01 mol / L glacial acetic acid-anhydrous ethanol mixed solution was prepared, in which anhydrous ethanol was used as the solvent and glacial acetic acid was used as the solute. This solution was then slowly added to the tetrabutyl titanate solution under stirring until the pH of the solution reached 4. The addition was stopped to obtain an acidic tetrabutyl titanate solution. The equal volume impregnation method was used to drop the mixture onto 10 g of clean nano-SiO 2 The surface was left at room temperature for 24 h, dried at 120 °C for 12 h, calcined at 500 °C for 5 h, and ground into powder to obtain TiO 2 -SiO 2 Support, of which TiO 2 The loading is 20%.
[0059] Weigh 0.3 g of niobium oxalate and dissolve it in 10 mL of deionized water, and disperse it ultrasonically for 5 min to obtain a clear niobium oxalate solution. Then weigh 0.2 g of gadolinium nitrate nonahydrate and dissolve it in the niobium oxalate solution, and disperse it ultrasonically for 5 min to obtain a clear Nb-Gd mixed solution. The mixed solution was dropped into 10 g of TiO by equal volume impregnation method. 2 -SiO 2 The surface of the carrier was left at room temperature for 24 h, dried at 120 °C for 12 h, and calcined at 500 °C for 5 h to obtain Nb-Gd / TiO 2 -SiO 2 Catalyst, Nb 2 O 5 The loading amount is 1.2%, Gd 2 O 3The loading was 1%.
[0060] Weigh 3.0 mL Nb-Gd / TiO 2 -SiO 2 The catalyst was loaded into a fixed bed reactor. Before the reaction, the catalyst was treated at 300°C and 50 mL / min nitrogen atmosphere for 3 hours to remove impurities remaining in the system and ensure that the reactants and products can pass through the reaction system smoothly. During the reaction, the formaldehyde feed rate was 0.05 mL / min, the isobutylene feed rate was 50 mL / min, the nitrogen flow rate was 20 mL / min, and the reaction temperature was 300°C. The obtained formaldehyde conversion rate was 92%, the isobutylene selectivity was 72%, and the isoprene yield was 45%.
[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for synthesizing isoprene, It is characterized in that The following steps are involved: Under the action of a catalyst, formaldehyde and isobutylene react to obtain isoprene; The catalyst comprises a carrier and a first transition metal oxide, a second transition metal oxide and a rare earth metal oxide supported on the carrier; The first transition metal and the second transition metal are different; The first transition metal oxide is TiO 2 ; The second transition metal is selected from Pd, Zr, Cs, Mo, V, Cu, Zn, Cr, Fe, Co or Ni.
2. The method for synthesizing isoprene according to claim 1, It is characterized in that The loading amount of the first transition metal is 5% to 50%; The loading amount of the second transition metal oxide is 0.1% to 10%; The loading amount of the rare earth metal oxide is 0.1% to 10%.
3. The method for synthesizing isoprene according to claim 2, It is characterized in that The loading amount of the first transition metal is 10% to 20%; The loading amount of the second transition metal oxide is 1% to 2%; The loading amount of the rare earth metal oxide is 1% to 2%.
4. The method for synthesizing isoprene according to claim 1, It is characterized in that The rare earth metal is selected from La, Ce, Rb, Pr, Gd, Er, Tm, Sm, Tb or Ho.
5. The method for synthesizing isoprene according to claim 1, It is characterized in that The carrier is selected from SiO 2 ,γ-Al 2 O 3 , MgO, CaO, MnO or BaO.
6. The method for synthesizing isoprene according to any one of claims 1 to 5, It is characterized in that The mass ratio of the formaldehyde, isobutylene and catalyst is (0.05-0.5):(50-150):(0.5-5).
7. A method for preparing a catalyst for use in the method for synthesizing isoprene according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step 1) mixing a titanium source solution and a carrier, and performing a first calcination; Step 2) Mixing a second transition metal source, a rare earth metal source and the product obtained in step 1), and performing a second calcination to obtain the catalyst.
8. The method for preparing the catalyst in the method for synthesizing isoprene according to claim 7, It is characterized in that The pH of the titanium source solution is 1-6.