A method for preparing vanadium oxide thin film for smart windows
Through the combination of dry etching and wet etching, the problems of transmittance, modulation efficiency and phase change temperature of vanadium oxide films in the field of smart windows have been solved, and flat and smooth film properties have been achieved, which is suitable for smart window applications.
Patent Information
- Application Number
- CN202310137379.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-20
AI Technical Summary
The existing technology is difficult to simultaneously meet the visible light transmittance, solar light modulation efficiency and phase change temperature requirements of vanadium oxide films in the field of smart windows. Moreover, the film has high roughness and cannot be directly applied to smart window coatings.
Dry etching technology is used, and SF6 is used for reactive ion etching of the VO2 film. The etching conditions are controlled to reduce the phase transition temperature, improve transmittance and optical performance, and are combined with wet etching to further optimize film performance.
The visible light transmittance and solar light modulation efficiency of the vanadium oxide film are achieved to meet the smart window standards, the phase change temperature is reduced, and the surface flatness of the film is improved, making it suitable for smart window applications.
Smart Images

Figure CN116395977B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of phase change materials, and in particular to a method for preparing a vanadium oxide film applied to a smart window. Background Art
[0002] With the development of economy, my country's demand for energy is increasing, and the contradiction between energy supply and demand is becoming increasingly apparent. Developing environmentally friendly new energy while achieving energy conservation is an effective way to solve the current problem. Among them, building energy consumption accounts for more than 40% of the global total energy consumption, which is a major energy loss, and the energy consumption of lighting, air conditioning, refrigeration and heating accounts for a large proportion of building energy consumption. From the perspective of building components, windows are the most energy-saving components in buildings. By developing smart materials as glass window coatings, smart windows can automatically adjust the solar energy intake according to changes in external temperature, thereby adjusting the room temperature and achieving energy conservation and environmental protection.
[0003] There are many types of vanadium oxide. In addition to at least 13 different phases such as V2O5, VO2, V2O3, VO, there are also many intermediate phases. The properties of vanadium oxide will also change with different components. There are large differences in the temperature coefficient of resistance and resistivity of vanadium oxide in different phases. Among the vanadium oxides in different physical phases, VO2 film has a high temperature coefficient of resistance and a low resistivity near room temperature, and can be used as a good thermal sensitive material in multiple technical fields.
[0004] In addition, VO2 is also a thermochromic material with phase change function, that is, when the external temperature changes, its physical properties (including optics, electricity, magnetism, etc.) will also change, which is suitable for the field of smart windows. The phase change temperature (Tc) of VO2 is 68°C. When the temperature is greater than 68°C, VO2 will undergo a reversible phase change, and its crystal structure will change from the monoclinic M phase to the tetragonal rutile R phase, and the infrared light will also change from high transmittance to high reflectivity, which can effectively reduce the indoor temperature. Moreover, during the thermochromic phase change process, the change is very rapid, and the film will not be destroyed in repeated reversible phase changes. Therefore, VO2 also has great application potential in many fields such as terahertz modulation, Mott transistors, chemical sensors, and optoelectronic devices.
[0005] Although a lot of research has been done on the thermochromic properties of VO2 thin films, there are still many problems to be solved in practical applications. In the field of smart windows, if VO2 thin films are used as smart window coatings, the following conditions need to be met:
[0006] (1) Visible light transmittance is large, T lum ≥40%, meeting lighting requirements;
[0007] (2) The solar light modulation efficiency is high, ΔT sol≥10%, meeting energy-saving requirements;
[0008] (3) The phase transition temperature is low, preferably Tc close to room temperature, which can effectively regulate solar energy intake;
[0009] (4) The film color is bright and comfortable.
[0010] In order to satisfy these four conditions at the same time, especially to make T lum ≥40% of simultaneous ΔT sol ≥10%, researchers conduct research work from multiple aspects.
[0011] Doping is the current mainstream method to reduce the phase transition temperature. It is common to achieve single element doping and co-doping of VO2 thin films. However, single element doping can only improve the thermochromic performance of a certain aspect of the film, and has little help in improving the overall thermochromic performance. Therefore, multi-element doping came into being. lum , ΔT sol 83% and 4.3% respectively. Similar to W-Mg co-doping, W-Sr co-doping and W-Zr co-doping also have ΔT sol The problem of small size and poor overall thermochromic performance. At present, some studies use magnetron sputtering, chemical vapor deposition, sol-gel and hydrothermal methods to improve the problem of poor overall thermochromic performance of VO2 thin films. Among these methods, the most widely used is reactive magnetron sputtering. Compared with other methods, reactive magnetron sputtering equipment is simple, easy to control, has a large coating area, and the obtained film has strong adhesion to the substrate. However, the VO2 thin film obtained by reactive magnetron sputtering has the problem of low transmittance, and it cannot be directly applied to the application conditions of smart window coatings. Summary of the invention
[0012] The inventor's previous research showed that wet etching of vanadium oxide thin films can improve visible light transmittance and sunlight modulation efficiency. However, the inventor's subsequent research showed that wet etching increases modulation by increasing surface holes. As the wet etching time increases, large and deep holes are formed on the surface of the film, which reduces the interconnection between particles and causes the phase transition temperature to rise. In addition, wet etching is greatly affected by temperature changes, and its etching rate varies greatly at different temperatures.
[0013] Dry etching is a technology that uses plasma to etch thin films. However, the current dry etching is mainly used for patterned etching of VO2. There is no literature reporting the use of dry etching to improve the phase change temperature or transmittance of VO2 thin films. This is mainly because the patterned etching scheme makes it difficult to accurately control the etching speed of VO2 thin films.
[0014] To solve the above problems, the present invention adopts dry etching, specifically, by controlling the etching conditions and removing the surface layer (the film is thinned, but the film surface is relatively flat and smooth) to improve the transmittance and change the film phase transition temperature and optical properties.
[0015] However, the inventors of the present invention found that not all etching gases can be used for vanadium oxide etching, and only under the technical solution of the present invention, that is, using SF6 to etch the vanadium oxide film, can the technical effect of lowering the phase change temperature and improving the visible light transmittance and solar light modulation efficiency be achieved.
[0016] For example, the inventors found that the etching speed of CF4 and CHF3 on vanadium oxide thin films was difficult to control, which may cause the surface of the film to be uneven (related to roughness). Excessive etching speed may even cause irreversible damage to the performance of the film. Finally, the effect of preparing vanadium oxide thin films was not ideal and was not suitable for preparing smart window coatings. Since the etching speed could not be controlled, the time to etch the same thickness of vanadium oxide thin films was different each time (used to calibrate the etching speed), so the etching method using gases such as CF4 and CHF3 was directly abandoned without making corresponding charts and data representations; the etching speed does not directly affect the visible light transmittance, solar light modulation efficiency, phase change temperature, etc., but in order to better control the etching thickness, the etching speed needs to be as slow as possible.
[0017] Therefore, the purpose of the present invention is to provide a method for preparing vanadium oxide thin films for use in smart windows, so as to solve the problems in the existing technology for preparing vanadium oxide thin films that the visible light transmittance and sunlight modulation efficiency cannot simultaneously meet the smart window use standards and the roughness of the prepared films is relatively high.
[0018] To achieve the above object, the present invention adopts the following technical solution:
[0019] A VO2 thin film is prepared on the surface of a substrate by magnetron sputtering, and then the VO2 thin film is dry-etched. The dry etching refers to reactive ion etching of the VO2 thin film with SF6. The etching process is more stable, the etching speed is constant, and the damage to the surface of the film is small. A vanadium oxide thin film with a smooth and uniform surface and adjustable thickness that can be used in smart windows is obtained.
[0020] The conditions of the reactive ion etching are as follows: the pressure in the chamber is 280-330 mT, the etching power is 15-20 W, the flow rate of SF6 is 40 sccm-60 sccm; further, the flow rate of SF6 is 50 sccm.
[0021] In the present invention, the reactive ion etching time is 1-7 minutes.
[0022] In some embodiments of the present invention, the reactive ion etching time is 2.5-7 minutes.
[0023] In some specific embodiments of the present invention, the conditions of reactive ion etching are: the chamber pressure is 300 mT, the etching power is 20 W, the flow rate of SF6 is 50 sccm, and the etching time is 6 min.
[0024] In some embodiments of the present invention, the VO2 film is further subjected to wet etching treatment, wherein the wet etching treatment refers to immersing the VO2 film in a nitric acid aqueous solution for 7-21 seconds;
[0025] Furthermore, the nitric acid aqueous solution is prepared by mixing nitric acid with twice the volume of water.
[0026] For example, in Example 2, samples 5, 6, 7, and 8, after dry and wet etching, have visible light transmittances of 49.20%, 56.11%, 63.16%, and 71.47%, respectively; and solar light modulation rates of 18.62%, 18.46%, 15.95%, and 14.56%, respectively; which are far higher than the preparation standards of smart windows.
[0027] In the present invention, the method of preparing a VO2 thin film on a substrate surface by magnetron sputtering includes the following steps: using a metal vanadium target as a sputtering target, performing low-temperature sputtering deposition on the substrate by DC reactive magnetron sputtering, and then performing a high-temperature in-situ annealing treatment in an oxygen-rich atmosphere to prepare a VO2 thin film.
[0028] In the present invention, the purity of the metallic vanadium is greater than 99.95%.
[0029] In the present invention, the sputtering includes two stages: a pre-sputtering stage and a sputtering stage.
[0030] During the pre-sputtering stage, the vacuum degree in the chamber of the magnetron sputtering device was adjusted to less than 1.7×10 -3 Pa, under the condition that the substrate holder rotates at a constant speed of 4 to 8 rpm, Ar is filled in for pre-sputtering.
[0031] During the sputtering stage, after the pre-sputtering is completed, O2 is filled in. After the pressure of the Ar and O2 mixed gas in the chamber is stabilized, the substrate holder is ensured to rotate at a constant speed of 4 to 8 rpm, and formal sputtering is carried out under the condition that the pressure in the chamber of the magnetron sputtering device is 0.91 Pa.
[0032] In the present invention, the pre-sputtering substrate temperature is 59-61° C., the Ar flow rate during the pre-sputtering process is 98-99 sccm, the current is 0.34 A, and the pre-sputtering time is 20 min.
[0033] In the present invention, the temperature of the sputtering substrate is 59-61° C., the flow rate of Ar during the sputtering process is 98-99 sccm, the flow rate of O2 is 1.9-2.2 sccm, the current is 0.34 A, and the sputtering time is 20 min-25 min.
[0034] In the present invention, the high temperature in-situ annealing treatment refers to annealing for 1 hour at a high temperature annealing substrate temperature of 400° C. with an O 2 flow rate of 1.4 to 1.6 sccm.
[0035] In the present invention, the substrate used is a quartz glass sheet. As a preferred solution, after the surface of the quartz glass sheet is cleaned, it is placed in the chamber of the magnetron sputtering device; wherein the cleaning process of the quartz glass sheet is as follows: firstly, the quartz glass sheet is placed in acetone for ultrasonic treatment to remove surface impurities, then placed in anhydrous ethanol for ultrasonic treatment to remove residual acetone, then placed in deionized water for ultrasonic treatment, and finally placed in anhydrous ethanol for storage; before the quartz glass sheet is placed in the chamber, it is blown dry with N2.
[0036] The reactive ion etching described in the present invention is a type of dry etching.
[0037] The present invention uses metal vanadium as a target, prepares a VO2 film by low-temperature sputtering deposition and high-temperature in-situ annealing, and adopts a reactive ion etching modification method to regulate its metal-insulator transition (MIT) performance, thereby preparing a vanadium oxide film whose visible light transmittance and solar light modulation efficiency meet the conditions of smart windows. Compared with the prior art, the vanadium oxide film prepared by this method obtains visible light transmittance, solar light modulation amplitude and phase transition temperature that meet the standards for use of smart windows. Compared with pure wet etching, the film thickness is more controllable and the roughness is also reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is the process flow chart of the present invention;
[0039] Figure 2 The transmittance-temperature curves of the sample 3 and sample 4 obtained in Example 1 and the vanadium oxide thin film obtained in Comparative Example 1 at 1100 nm;
[0040] FIG3 is the first order differential and Gaussian fitting curve of the transmittance-temperature curves of Sample 3 and Sample 4 obtained in Example 1 and the vanadium oxide thin film obtained in Comparative Example 1 at 1100 nm;
[0041] Figure 4 Visible-near infrared transmission spectra of sample 3 and sample 4 obtained in Example 1 and the vanadium oxide film obtained in Comparative Example 1 at room temperature and high temperature.
[0042] Figure 5The transmittance-temperature curves of the vanadium oxide thin films obtained in Example 2, Sample 5, Sample 6, Sample 7, Sample 8 and Comparative Example 1 and Comparative Example 2 at 1100 nm are shown;
[0043] 6 is the first order differential and Gaussian fitting curve of the transmittance-temperature curves of Samples 5, 6, 7, and 8 obtained in Example 2 and the vanadium oxide thin film obtained in Comparative Example 2 at 1100 nm;
[0044] Figure 7 Visible-near infrared transmission spectra of the vanadium oxide thin films obtained in samples 5, 6, 7, and 8 obtained in Example 2 and comparative examples 1 and 2 at room temperature and high temperature;
[0045] Figure 8 AFM characterization images of Sample 3 and Sample 4 prepared in Example 1, Sample 5, Sample 6, Sample 7, Sample 8 prepared in Example 2, and Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0046] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but the description is not intended to limit the present invention.
[0047] Example 1
[0048] like Figure 1 As shown, a method for preparing a vanadium oxide thin film for use in a smart window comprises the following steps:
[0049] (1) Use quartz glass as the substrate and clean it before the experiment to keep it clean. Specifically: first clean the substrate with detergent, then clean the foam with clean water and deionized water, then immerse the substrate in acetone, ethanol, and deionized water respectively, and clean it in ultrasound for more than 30 minutes each time. After cleaning, store it in ethanol and blow it dry with N2 with a purity of ≥99.999% before use.
[0050] (2) Using a metal vanadium target with a purity of more than 99.95% as the target material, the substrate is sputtered by a DC reactive magnetron sputtering method:
[0051] Sputtering is divided into two stages: pre-sputtering and sputtering:
[0052] Pre-sputtering stage: adjust the vacuum degree in the chamber of the CK-3 magnetron sputtering device to less than 1.7×10 -3 Pa, the substrate holder is rotated at a constant speed of 4-8 rpm, and Ar is filled for pre-sputtering. The substrate temperature for pre-sputtering is 60°C, the Ar flow rate is 98 sccm, and the current is 0.34 A. Under this condition, the pre-sputtering time is 20 minutes.
[0053] Sputtering stage: After the pre-sputtering is completed, O2 is filled in. After the pressure of the Ar and O2 mixed gas in the chamber is stable, the substrate holder is rotated at a constant speed of 4 to 8 rpm, and the formal sputtering is carried out under the condition that the pressure in the chamber of the CK-3 magnetron sputtering device is 0.91 Pa. The formal sputtering substrate temperature is 60°C, the flow rate of Ar is 98 sccm, the flow rate of O2 is 2 sccm, the sputtering current is 0.34A, and the sputtering time is 20 minutes under this condition.
[0054] (3) The VO2 film is subjected to high-temperature in-situ annealing in an oxygen-rich atmosphere. The substrate temperature for the in-situ annealing is 400°C. During the annealing process, the O2 flow rate is 15 sccm. Under this condition, the annealing is performed for 1 hour.
[0055] (4) The prepared VO2 film is etched in a reactive ion etcher. During the etching process, different samples are obtained by selecting different etching parameters. The vanadium oxide film samples prepared in this embodiment include sample 1, sample 2, sample 3, and sample 4. As shown in Table 1, the thickness of sample 1 and sample 3 tends to be consistent, and the thickness of sample 2 and sample 4 tends to be consistent. By comparing the changes in visible light transmittance, solar light modulation efficiency, and phase transition temperature of vanadium oxide film samples of the same thickness after etching, better etching conditions are selected.
[0056] Table 1
[0057] Thickness(nm) Sample 1 109.1 Sample 2 90.3 Sample 3 107.8 Sample 4 87.18
[0058] Among them, the etching parameters of sample 1 and sample 2 are: the chamber pressure is 300mT, the RIE FWD is 50W (etching power), the flow rate of SF6 is 50sccm, and the etching time is 2.5min and 3min respectively, to obtain vanadium oxide thin film samples 1 and sample 2.
[0059] The etching parameters of sample 3 and sample 4 are as follows: the chamber pressure is 300mT, the RIE FWD is 20W, the flow rate of SF6 is 50sccm, and the etching time is 6min and 7min respectively; vanadium oxide thin film samples 3 and 4 are obtained.
[0060] Comparative Example 1
[0061] (1) Use quartz glass as the substrate and clean it before the experiment to keep it clean. Specifically: first clean the substrate with detergent, then clean the foam with clean water and deionized water, then immerse the substrate in acetone, ethanol, and deionized water respectively, and clean it in ultrasound for more than 30 minutes each time. After cleaning, store it in ethanol and blow it dry with N2 with a purity of ≥99.99% before use.
[0062] (2) Using a metal vanadium target with a purity of more than 99.95% as the target material, the substrate is sputtered by a DC reactive magnetron sputtering method:
[0063] Sputtering is divided into two stages: pre-sputtering and sputtering:
[0064] Pre-sputtering stage: adjust the vacuum degree in the chamber of the CK-3 magnetron sputtering device to less than 1.7×10 -3 Pa, the substrate holder is rotated at a constant speed of 4-8 rpm, and Ar is filled for pre-sputtering. The substrate temperature for pre-sputtering is 60°C, the Ar flow rate is 98 sccm, and the current is 0.34 A. Under this condition, the pre-sputtering time is 20 minutes.
[0065] Sputtering stage: After the pre-sputtering is completed, O2 is filled in. After the pressure of the Ar and O2 mixed gas in the chamber is stable, the substrate holder is rotated at a constant speed of 4 to 8 rpm, and the formal sputtering is carried out under the condition that the pressure in the chamber of the CK-3 magnetron sputtering device is 0.91 Pa. The formal sputtering substrate temperature is 60°C, the flow rate of Ar is 98 sccm, the flow rate of O2 is 2 sccm, the sputtering current is 0.34A, and the sputtering time is 20 minutes under this condition.
[0066] (3) The VO2 film was subjected to high-temperature in-situ annealing in an oxygen-rich atmosphere. The substrate temperature for the in-situ annealing was 400°C. During the annealing process, the O2 flow rate was 15 sccm. Under this condition, the sample of comparative example 1 was obtained by annealing for 1 hour.
[0067] The optical phase change properties of the vanadium oxide thin film samples 1, 2, 3, 4 and comparative example 1 were measured by Fourier transform infrared spectrometer, as shown in Table 2:
[0068] Table 2
[0069]
[0070]
[0071] Table 1 and Figure 2 Figure 3 Figure 4 It can be seen that the phase transition temperatures of samples 1 to 4 obtained after reactive ion etching are reduced, and the phase transition temperature of sample 3 is as low as 50.56° C., which is 6.73° C. lower than the phase transition temperature of the sample in comparative example 1.
[0072] It can be seen that the vanadium oxide film obtained by the preparation method of this embodiment is more suitable for application in the field of smart windows.
[0073] The visible light transmittance and solar light modulation efficiency of vanadium oxide thin film sample 1, sample 2, sample 3, sample 4 and comparative example 1 were tested at 380nm-2500nm, and the test results are shown in Table 3:
[0074] Table 3
[0075] Visible light transmittance (%) Solar light modulation efficiency (%) Sample 1 41.93 11.04 Sample 2 42.71 10.50 Sample 3 40.52 12.18 Sample 4 43.45 11.2 Comparative Example 1 Sample 21.13 17.19
[0076] Combined with Table 2, Figure 2 Figure 3 Figure 4 It can be seen that in the 380nm-2500nm band, as the visible light transmittance increases, the solar light modulation efficiency gradually decreases. Samples 1 to 4 all meet the requirements of visible light transmittance ≥40% and solar light modulation efficiency ≥10%. However, when comparing samples 1 and 2 with samples 3 and 4, when the visible light transmittance and solar light modulation efficiency are roughly the same, the etching parameters of samples 3 and 4 can reduce the phase change temperature more, which is better than the etching parameters of samples 1 and 2. This shows that the MIT performance of vanadium oxide film can be effectively regulated by reactive ion etching, and the optimization of parameters can make the final vanadium oxide film better used in the field of smart windows.
[0077] The XPS spectra of vanadium oxide film sample 3, sample 4 and comparative example 1 were tested respectively, and the V 4+ 、V 5+ The composition ratio of the calculated results is shown in Table 4:
[0078] Table 4
[0079] <![CDATA[V 4+ (%)]]> <![CDATA[V 5+ (%)]]> Sample 3 47.22 52.78 Sample 4 46.79 53.21 Comparative Example 1 Sample 54.58 45.42
[0080] From the analysis, it is known that the phase transition temperature is affected by many factors, such as particle size, particle shape, grain boundary, surface morphology, etc. The reasons for its reduction may be: 1. V 4+ The relative fraction of VO2 decreases; 2. The surface local defects in VO2 can effectively promote the heterogeneous nucleation of MIT, making the phase transition of the film easier to occur and thus reducing its overall phase transition temperature; 3. The phase transition temperature of VO2 film varies with the particle size. 4+ A decrease in the relative fraction of will also result in a decrease in the solar light modulation efficiency.
[0081] The AFM spectra of the vanadium oxide film sample 3, sample 4 and the vanadium oxide film of comparative example 1 were tested respectively. Figure 8 As shown, the root mean square roughness of the sample is calculated, and the calculation results are shown in Table 5:
[0082] Table 5
[0083] Root mean square roughness Rq Sample 3 6.32 Sample 4 14.5 Comparative Example 1 Sample 8.58
[0084] It can be seen from Table 4 that reactive ion etching treatment within a certain period of time will reduce the root mean square roughness of the sample and make the sample surface smoother, but a longer etching time will increase the root mean square roughness again.
[0085] Example 2
[0086] Steps (1) to (3) of this embodiment are the same as those of embodiment 1 and are not described in detail here. The difference from embodiment 1 is that after the reactive ion etching is performed, the steps are as follows:
[0087] (4) The VO2 film prepared in step (3) is etched in a reactive ion etcher. During the etching process, the chamber pressure is 300 mT, the RIE FWD is 20 W, and the SF6 flow rate is 50 sccm. Under these conditions, etching is performed for 1 min.
[0088] (5) Prepare a nitric acid solution with a ratio of HNO3:H2O=60ml:120ml, add a magnetic stirrer, stir thoroughly with a stirring rod, and then let it stand. Wait for the solution to cool before wet etching. During the wet etching process, place the sample on a custom substrate holder, immerse the substrate holder in the solution, and etch for 7s, 14s, 18s, and 21s, respectively, to obtain Sample 5, Sample 6, Sample 7, and Sample 8.
[0089] Comparative Example 2
[0090] Steps (1) to (3) of this comparative example are the same as those of comparative example 1 and are not described in detail here. The difference from comparative example 1 is that the following step is added:
[0091] (4) Prepare a nitric acid solution with a ratio of HNO3:H2O=60ml:120ml, add a magnetic stirrer, stir thoroughly with a stirring rod, and then let it stand, wait for the solution to cool, and then perform wet etching. During the wet etching process, place the sample on a custom substrate holder, immerse the substrate holder in the solution, and etch for 15 seconds to obtain Comparative Example 2.
[0092] The optical phase change properties of vanadium oxide thin film samples 5, 6, 7, 8 and comparative examples 1 and 2 were measured by Fourier transform infrared spectrometer, as shown in Table 6:
[0093] Table 6
[0094] Phase transition temperature (°C) Cooling phase transition temperature / ℃ Phase change temperature / ℃ Sample 5 61.95 45.70 53.83 Sample 6 65.53 46.65 56.09 Sample 7 62.83 49.80 56.32 Sample 8 64.52 48.08 56.30 Comparative Example 1 Sample 64.40 50.18 57.29 Comparative Example 2 Sample 67.88 51.68 59.78
[0095] Combined with Table 5, Figure 5 Figure 6 Figure 7 It can be seen that the vanadium oxide thin film sample prepared in Example 2 not only reduces the phase transition temperature, but also effectively improves the problem of increased phase transition temperature caused by large and deep holes on the surface of the film after wet etching alone in the prior art, which makes the particles less connected to each other or even almost isolated, making it less likely for phase change to occur. The phase transition temperature of Sample 5 is as low as 53.83°C, which is 3.46°C lower than that of the sample in Comparative Example 1 and 5.95°C lower than that of the sample in Comparative Example 2.
[0096] The visible light transmittance and solar light modulation efficiency of Sample 5, Sample 6, Sample 7, Sample 8 and Comparative Examples 1 and 2 were tested at 380nm-2500nm, and the test results are shown in Table 7.
[0097] Table 7
[0098] Visible light transmittance (%) Solar light modulation efficiency (%) Sample 5 49.20 18.62 Sample 6 56.11 18.46 Sample 7 63.16 15.95 Sample 8 71.47 14.56 Comparative Example 1 Sample 21.03 17.19 Comparative Example 2 Sample 46.96 18.21
[0099] Combined with Table 6, Figure 5 Figure 6 Figure 7 It can be seen that the vanadium oxide thin film samples prepared in Example 2 meet the requirements of visible light transmittance ≥40% and solar light modulation efficiency ≥10% in the 380nm-2500nm band. Not only are the visible light transmittance and solar light modulation efficiency greatly improved, but the visible light transmittance is not improved at the expense of solar light modulation efficiency. The vanadium oxide thin film samples are dry-etched for the same time and then wet-etched for different times. In a shorter wet etching time, the visible light transmittance and solar light modulation efficiency can be improved at the same time, which is a significant improvement on the basis of the existing technology.
[0100] The XPS spectra of vanadium oxide film samples 5, 6, 7, 8 and the comparative example vanadium oxide film were tested respectively, and the V 4+ 、V 5+ The composition ratio of the calculated results is shown in Table 8:
[0101] Table 8
[0102]
[0103]
[0104] From the analysis, it is known that compared with simple wet etching, dry-wet etching can significantly increase V 4+ The relative fraction of VO2 reduces the oxidation state of the VO2 film, thereby reducing the phase transition temperature and improving the solar light modulation efficiency.
[0105] The SEM and AFM spectra of the vanadium oxide thin film samples 5, 6, 7, 8 and comparative example 1 were tested respectively. Figure 8 As shown, the thickness and root mean square roughness of the sample are calculated, and the calculation results are shown in Table 9:
[0106] Table 9
[0107] Thickness(nm) Root mean square roughness Rq(nm) Sample 3 107.8 6.32 Sample 4 87.18 14.5 Sample 5 152 10.4 Sample 6 121 11.5 Sample 7 103 13.5 Sample 8 88.3 14.8 Comparative Example 1 Sample 200 8.58 Comparative Example 2 Sample 126 26.7
[0108] As shown in Table 8, pure wet etching will increase the RMS roughness of the sample (Comparative Example 1 and Comparative Example 2); pure dry etching will reduce the RMS roughness of the sample to a certain extent, and the RMS roughness will increase again after exceeding the etching limit (Comparative Example 1 and Samples 3 and 4). Comparing the two groups of Samples 3 and 7 and Samples 4 and 8, when etching to approximately the same thickness, the sample roughness obtained by pure dry etching is lower than that obtained by dry-wet etching; comparing Sample 6 and Comparative Example 2, when etching to approximately the same thickness, the sample roughness obtained by dry-wet etching is lower and smoother than that obtained by pure wet etching.
[0109] From this analysis, it can be concluded that the roughness obtained by dry-wet etching is between pure dry etching and pure wet etching. At the same time, dry-wet etching can reduce the phase change temperature and improve the visible light transmittance and solar modulation efficiency. It achieves a good balance among various parameters and obtains a flat and smooth film that is more suitable for smart windows.
[0110] In summary, it can be seen that the vanadium oxide film obtained by the preparation method provided by the present invention greatly improves the visible light transmittance of the vanadium oxide film at 380-2500nm, and better maintains the solar light modulation efficiency of the film, while effectively reducing the phase change temperature and roughness of the film, making the film smoother and smoother, and having more application prospects in the field of smart windows.
[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a vanadium oxide thin film for use in smart windows, characterized in that: A VO2 film is prepared on the surface of a substrate by magnetron sputtering, and then the VO2 film is dry-etched; the dry etching is to use SF6 to perform reactive ion etching on the VO2 film, so that the etching process is more stable, the etching speed is constant, and the damage to the film surface is small, so as to obtain a vanadium oxide film with a smooth and uniform surface, adjustable thickness, and applicable to smart windows; wherein, the use of SF6 to etch the vanadium oxide film can reduce the phase transition temperature, while improving the visible light transmittance and solar light modulation efficiency; The conditions of the reactive ion etching are: the chamber pressure is 280-330mT, the etching power is 15-20W, and the flow rate of SF6 is 40sccm-60sccm; The method further includes wet etching the dry-etched VO2 film, wherein the wet etching process refers to immersing the VO2 film in a nitric acid aqueous solution for 7-21 seconds; the wet etching process of the dry-etched VO2 film includes: Perform dry etching for a certain period of time and then perform wet etching for a short time; wet etching after dry etching can significantly increase V 4+ The relative fraction of VO2 reduces the oxidation state of the VO2 film, thereby reducing the phase transition temperature and improving the solar light modulation efficiency.
2. The method according to claim 1, characterized in that The reactive ion etching time is 1-7min.
3. The method according to claim 2, characterized in that The conditions of reactive ion etching are: the chamber pressure is 300mT, the etching power is 20W, and the flow rate of SF6 is 50sccm.
4. The method according to any one of claims 1 to 3, characterized in that: Aqueous nitric acid is prepared by mixing nitric acid with twice its volume of water.
5. The method according to claim 1, characterized in that The method of preparing a VO2 thin film on a substrate surface by magnetron sputtering includes the following steps: A metal vanadium target is used as a sputtering target, a DC reactive magnetron sputtering method is used to perform low-temperature sputtering deposition on a substrate, and then a high-temperature in-situ annealing treatment is performed in an oxygen-rich atmosphere to prepare a VO2 thin film; the purity of the metal vanadium is greater than 99.95%.
6. The method according to claim 5, characterized in that The sputtering includes two stages: a pre-sputtering stage and a sputtering stage; In the pre-sputtering stage, the vacuum degree in the chamber of the magnetron sputtering device is adjusted to less than 1.7×10 -3 Pa, under the condition that the substrate holder rotates at a constant speed of 4 to 8 rpm, Ar is filled for pre-sputtering; In the sputtering stage, after the pre-sputtering is completed, O2 is filled in. After the pressure of the Ar and O2 mixed gas in the chamber is stabilized, the substrate holder is ensured to rotate at a constant speed of 4 to 8 rpm, and formal sputtering is carried out under the condition that the pressure in the chamber of the magnetron sputtering device is 0.91 Pa.
7. The method according to claim 6, characterized in that The pre-sputtering substrate temperature is 59-61° C., the Ar flow rate during the pre-sputtering process is 98-99 sccm, the current is 0.34 A, and the pre-sputtering time is 20 min.
8. The method according to claim 6, characterized in that The temperature of the sputtering substrate is 59-61° C., the flow rate of Ar during the sputtering process is 98-99 sccm, the flow rate of O2 is 1.9-2.2 sccm, the current is 0.34 A, and the sputtering time is 20 min-25 min.
9. The method according to claim 6, characterized in that The high temperature in-situ annealing process refers to annealing for 1 hour under the conditions of an O2 flow rate of 1.4 to 1.6 sccm and a high temperature annealing substrate temperature of 400°C.
10. The method according to claim 1, characterized in that The substrate is a quartz glass sheet; after the surface of the quartz glass sheet is cleaned, it is placed in the chamber of the magnetron sputtering device; the cleaning process of the quartz glass sheet is as follows: first, the quartz glass sheet is placed in acetone for ultrasonic treatment to remove surface impurities, then placed in anhydrous ethanol for ultrasonic treatment to remove residual acetone, and then placed in deionized water for ultrasonic treatment, and finally placed in anhydrous ethanol for storage; the quartz glass sheet is blown dry with N2 before being placed in the chamber.