A method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio
Through improved chemical vapor deposition equipment and rare earth chelate vapor phase heating system, drilling and MCVD deposition lathe shrinking process, the processing problem of large core diameter rare earth doped optical fiber preforms has been solved, and the uniformity and uniformity of the rare earth doped core have been improved. Production efficiency, achieving efficient preparation of large core-to-cladding ratio optical fiber preforms.
Patent Information
- Application Number
- CN202211647314.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-21
AI Technical Summary
In the existing technology, the core package used to prepare large-core-diameter rare-earth-doped optical fiber preforms is relatively small, difficult to process, has poor distribution uniformity of rare-earth ions, and requires long-term solution soaking and dehydration processes, which can easily lead to optical fiber core loss.
Using improved chemical vapor deposition equipment combined with a rare earth chelate vapor phase heating system, a conventional core-to-cladding ratio rare earth-doped optical fiber preform is first prepared, drilled to form a thin-diameter core rod, and then shrunk through an MCVD deposition lathe to form a large core-to-cladding ratio. Rare earth-doped optical fiber preform improves doping uniformity and production efficiency.
The efficient preparation of rare earth-doped optical fiber preforms with a large core-to-cladding ratio is achieved, the purity and uniformity of the rare earth-doped core are improved, the processing difficulty and core loss are reduced, and the preparation time is shortened.
Smart Images

Figure CN116409923B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of special optical fiber preforms, and in particular to a method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio. Background Art
[0002] Compared with traditional CO2 lasers and solid-state lasers, fiber lasers have the advantages of high electro-optical conversion efficiency, good beam quality, and small footprint, which has promoted revolutionary changes in the laser market and has been widely used in industrial manufacturing, medical treatment, military defense and other fields. At present, fiber lasers are developing towards higher power, and industrial equipment equipped with high-power fiber lasers ranging from kilowatts to tens of kilowatts will become the mainstream equipment in the high-end manufacturing industry. Rare earth-doped fiber is the core component of fiber lasers. Large-core rare earth-doped fiber can generate large mode field gain and achieve high-power laser output. Through certain design, the output power can reach the 10,000-watt level, which is the key factor in determining the high-power output of fiber lasers. At present, industrial high-power continuous fiber lasers mostly use large-mode field double-clad ytterbium-doped fiber, and high-power lasers are obtained by combining multiple single modules. In the laser structure design, key components such as gain fiber, high / low reflection grating, (n+1)×1 signal / pump coupler are mainly involved. The pump fiber used in the (n+1)×1 signal / pump coupler adopts a rare earth-doped fiber with a large core-to-shell ratio. After pretreatment, the input signal fiber is connected to the subsequent optical path structure by forming an input fiber bundle with multiple tapered large core-to-shell ratio pump fibers. The large core-to-shell ratio pump fiber can be directly arranged closely around the periphery of the pretreated input signal fiber, or first tapered to a set diameter, and then closely arranged around the periphery of the input signal fiber. Therefore, the rare earth-doped fiber with a large core-to-shell ratio is very important for the key components of the high-power continuous fiber laser structure. Common large core-to-shell ratio rare earth-doped fibers include 105 / 125μm, 200 / 220μm, and 220 / 242μm rare earth-doped fibers, using a large core-to-shell ratio fiber structure with a core-to-shell ratio of 21:25 and 10:11.
[0003] The Chinese patent publication number is CN102108008A, and the publication date is June 29, 2011. The invention is named as a method for manufacturing a large-size rare earth element doped optical fiber preform. It discloses the use of a liquid phase doping method to prepare a rare earth doped core rod, the use of a vapor phase axial deposition (VAD) technology to deposit a powder core layer, the prepared core layer powder is immersed in a mixed solution containing rare earth elements and co-doping substances, and vitrified in a high-temperature furnace to form a core layer of a rare earth element optical fiber preform. Then, the outer cladding powder is deposited outside the core layer of the rare earth element optical fiber preform and vitrified at high temperature to form a cladding, or a glass tube is used to form a cladding outside the core layer of the rare earth doped optical fiber preform as a cladding, thereby forming a large core cladding optical fiber preform. The disadvantage of this method is that the rare earth ions are poorly distributed uniformly in the core when the rare earth doped optical fiber preform is prepared by liquid phase doping, and the purity of the configured rare earth element solution is about 10 times lower than that of the rare earth chelate. The preform preparation process requires at least 12 hours of long-term solution immersion to complete the doping process, and must go through a dehydration process. If any moisture remains, it will lead to an increase in subsequent optical fiber core loss. Summary of the invention
[0004] In view of the technical problems that the core package of the optical fiber preform is relatively small and the processing is difficult in the existing methods for preparing large core diameter rare earth doped optical fibers, the present invention provides a method for preparing a rare earth doped optical fiber preform with a large core package ratio, using an improved chemical vapor deposition device combined with a rare earth chelate gas phase heating system, first preparing a conventional core package ratio rare earth doped optical fiber preform, and drilling a hole in the middle of the rare earth doped optical fiber preform to remove it. A new quartz reaction tube is connected to the MCVD deposition lathe again, and the core of the preform is deposited in the same way. The taken out rare earth doped thin diameter core rod is placed in the middle of the quartz reaction tube, and then the rod is shrunk to form a rare earth doped optical fiber preform with a large core package ratio. The problem of preparing large core diameter rare earth doped optical fibers is solved from the preform preparation stage, the difficulty of preform processing is reduced, and at the same time, the doping uniformity of the rare earth doped core is improved and the optical fiber production efficiency is improved.
[0005] The technical solution adopted by the present invention is: a method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio, the steps of which are as follows:
[0006] Step 1, clean the quartz reaction tube and connect it to the MCVD deposition lathe, heat the rare earth chelate to the set temperature, use the hydrogen-oxygen flame to heat the quartz reaction tube, start the core layer deposition program, introduce the rare earth chelate in the gas state into the quartz reaction tube together with the SiCl4, POCl3, AlCl3, He, and O2 reaction material gases, set the number of deposited core layers, and perform the preform core deposition. After the core deposition is completed, increase the hydrogen-oxygen flame temperature to start the rod shrinking process. When the inner diameter of the quartz reaction tube is reduced to 2mm-3mm, the pressure in the tube is set to a negative value, and the quartz reaction tube is shrunk into a rare earth-doped optical fiber preform;
[0007] Step 2, placing the prepared rare earth-doped optical fiber preform in a drilling lathe, drilling the rare earth-doped core in the middle of the rare earth-doped optical fiber preform and taking it out as a whole to form a rare earth-doped thin-diameter core rod, and fusing a quartz rod with a diameter larger than that of the rare earth-doped thin-diameter core rod at both ends as a support rod;
[0008] Step 3, using hydrogen-oxygen flame to perform high-temperature flame polishing on the rare earth-doped thin-diameter core rod of the welding support rod to heal small surface defects;
[0009] Step 4, reconnect a new quartz reaction tube to the MCVD deposition lathe, and according to the method of step 1, introduce the rare earth chelate in gas state into the quartz reaction tube together with SiCl4, POCl3, AlCl3, He, and O2 reaction material gases again, set the number of deposited core layers, and perform preform core deposition. After the core deposition is completed, increase the oxyhydrogen flame temperature to start the rod shrinking process. When the inner diameter of the quartz reaction tube is reduced and larger than the diameter of the rare earth-doped thin-diameter core rod, reduce the oxyhydrogen flame temperature, and move the oxyhydrogen flame torch to the right end of the quartz reaction tube. Put the rare earth-doped thin-diameter core rod of the fused support rod processed in step 3 from the left side of the quartz reaction tube into the center of the quartz reaction tube, and fix the support rod on the support tube and tail tube on the MCVD lathe to keep synchronous rotation;
[0010] Step 5, raising the temperature of the hydrogen-oxygen flame again, setting the pressure in the quartz reaction tube to a negative value, shrinking the quartz reaction tube and the rare earth-doped thin-diameter core rod together into a solid preform, thereby preparing a rare earth-doped optical fiber preform with a large core-to-wrapper ratio.
[0011] The rare earth chelate described in step 1 is heated to a set temperature of 110° C. to 240° C.
[0012] In step 1, the number of deposited core layers is set to 15-20, forming a core-to-shell ratio of 1:3.
[0013] The rare earth-doped thin-diameter core rod in step 2 is 360 mm in length, and the rare earth-doped thin-diameter core rod is subjected to high-temperature polishing treatment.
[0014] In step 2, the rare earth-doped core in the middle of the rare earth-doped optical fiber preform is drilled and removed as a whole, with the center position of the rare earth-doped core in the middle of the rare earth-doped optical fiber preform as the center of the circle, and a drill bit with a size equal to the diameter of the rare earth-doped core is used to remove it.
[0015] As described in step 4, the number of deposited core layers is set to 20-30 layers.
[0016] As described in step 4, the inner diameter of the quartz reaction tube is reduced to 2 mm to 3 mm larger than the diameter of the rare earth-doped thin-diameter core rod.
[0017] The rare earth-doped optical fiber preform with a large core-to-clad ratio described in step 5 has a core-to-clad ratio of 21:25 or 10:11.
[0018] The beneficial effects of the present invention are as follows: through the technical solution described in the present invention, MCVD can be used to improve vapor deposition equipment and a vapor phase doping method can be used to prepare a rare earth-doped optical fiber preform, and a rare earth chelate with a purity of 99.999% is used as a raw material, thereby improving the doping uniformity and purity of the rare earth-doped core layer, avoiding the introduction of moisture during the preparation process, reducing the core loss of the subsequent optical fiber, and the overall preparation time of the preform can be controlled within 6 hours, thereby improving production efficiency.
[0019] The prepared large core-to-encapsulation ratio rare earth doped optical fiber preform can have a core-to-encapsulation ratio of 21:25 or 10:11. The method of the present invention can effectively solve the problem that the current improved chemical vapor deposition preparation process cannot prepare large core-to-encapsulation ratio optical fiber preform, and provide a solution for the development of large core-to-encapsulation ratio rare earth doped optical fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the rare earth-doped optical fiber preform in the present invention;
[0021] Figure 2 A schematic diagram of a rare earth-doped thin-diameter core rod in the present invention;
[0022] Figure 3 A schematic diagram of the connection between the rare earth-doped thin-diameter core rod and the support rod in the present invention;
[0023] Figure 4 This is a schematic diagram of placing a rare earth-doped thin-diameter core rod in a quartz reaction tube in the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose and technical solution of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0025] The present invention provides a method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio, comprising the following steps:
[0026] Step 1. Clean the quartz reaction tube with the size of 25mm*2mm*600mm and connect it to the MCVD deposition lathe, run the rare earth chelate gas phase heating system, and heat the rare earth chelate to the set temperature of 200°C. At the same time, use the hydrogen-oxygen flame to heat the quartz reaction tube to about 2000°C, start the core layer deposition program, and introduce the rare earth chelate in the gas state into the quartz reaction tube together with the SiCl4, POCl3, AlCl3, He, and O2 reaction material gases. Set the number of deposition layers to 15 layers. After completing the core deposition, increase the hydrogen-oxygen flame temperature to about 2200°C and start the rod shrinking process. When the inner diameter of the quartz reaction tube is about 2.5mm, set the pressure in the tube to a negative value, and shrink the quartz reaction tube into a rare earth-doped optical fiber preform 1, as shown in FIG. Figure 1 As shown in the figure, the core diameter is 4.5mm, the preform rod diameter is 13.8mm, and the core-to-wrapper ratio is about 1:3 as tested by the PK2600 optical fiber preform refractive index analyzer.
[0027] Step 2: Place the rare earth-doped optical fiber preform rod 1 in a drilling lathe, select a hollow drill bit with a diameter of 4.5 mm, drill a hole with the center of the rare earth-doped core as the center, and take out a rare earth-doped thin-diameter core rod 2 with a length of 360 mm. Figure 2 As shown. A quartz rod 3 with a diameter of 8 mm is welded to each end of the rare earth-doped thin-diameter core rod 2 as a support rod. Figure 3 shown.
[0028] Step 3: Use hydrogen-oxygen flame to perform high-temperature flame polishing on the removed rare earth-doped thin-diameter core rod 2 to heal small surface defects.
[0029] Step 4. Reconnect a new quartz reaction tube 4 of 25mm*2mm*400mm size to the MCVD deposition lathe. According to the method in step 1, the rare earth chelate in gas state is introduced into the quartz reaction tube together with SiCl4, POCl3, AlCl3, He, and O2 reaction material gases again, and the number of deposition layers is set to 25. After the core deposition is completed, the temperature of the oxyhydrogen flame is increased to about 2200°C to start the rod shrinking process. When the inner diameter of the quartz reaction tube is reduced to about 7mm, which is larger than the diameter of the rare earth-doped thin-diameter core rod 2 by 2.5mm, the temperature of the oxyhydrogen flame is lowered to 1300°C, and the oxyhydrogen flame torch is moved to the right end of the quartz reaction tube. The rare earth-doped thin-diameter core rod of the welded support rod processed in step 3 is placed into the quartz reaction tube from the left side, and the rare earth-doped thin-diameter core rod is adjusted to the center of the quartz reaction tube. The support rod 3 is fixed on the support tube 5 and the tail tube 6 on the MCVD lathe. Figure 4 As shown, keep rotating synchronously.
[0030] Step 5, raise the temperature of the hydrogen-oxygen flame to 2200°C again, set the pressure in the quartz reaction tube to a negative value, shrink the quartz reaction tube and the rare earth-doped thin-diameter core rod 2 together into a solid preform, thereby preparing a rare earth-doped optical fiber preform with a large core-to-package ratio. Tested by the PK2600 optical fiber preform refractive index analyzer, the core diameter is 11.35mm, the preform rod diameter is 14.59mm, and the core-to-package ratio is about 21:25, which can meet the development of 105 / 125μm rare earth-doped active optical fiber.
Claims
1. A method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio, characterized in that: Here are the steps: Step 1, clean the quartz reaction tube and connect it to the MCVD deposition lathe, heat the rare earth chelate to the set temperature, use the hydrogen-oxygen flame to heat the quartz reaction tube, start the core layer deposition program, introduce the rare earth chelate in the gas state into the quartz reaction tube together with the SiCl4, POCl3, AlCl3, He, and O2 reaction material gases, set the number of deposited core layers, and perform the preform core deposition. After the core deposition is completed, increase the hydrogen-oxygen flame temperature to start the rod shrinking process. When the inner diameter of the quartz reaction tube is reduced to 2mm-3mm, the pressure in the tube is set to a negative value, and the quartz reaction tube is shrunk into a rare earth-doped optical fiber preform; Step 2, placing the prepared rare earth-doped optical fiber preform in a drilling lathe, drilling the rare earth-doped core in the middle of the rare earth-doped optical fiber preform and taking it out as a whole to form a rare earth-doped thin-diameter core rod, and fusing a quartz rod with a diameter larger than that of the rare earth-doped thin-diameter core rod at both ends as a support rod; Step 3, using hydrogen-oxygen flame to perform high-temperature flame polishing on the rare earth-doped thin-diameter core rod of the welding support rod to heal small surface defects; Step 4, reconnect a new quartz reaction tube to the MCVD deposition lathe, and according to the method of step 1, introduce the rare earth chelate in gas state into the quartz reaction tube together with SiCl4, POCl3, AlCl3, He, and O2 reaction material gases again, set the number of deposited core layers, and perform preform core deposition. After the core deposition is completed, increase the oxyhydrogen flame temperature to start the rod shrinking process. When the inner diameter of the quartz reaction tube is reduced and larger than the diameter of the rare earth-doped thin-diameter core rod, reduce the oxyhydrogen flame temperature, and move the oxyhydrogen flame torch to the right end of the quartz reaction tube. Put the rare earth-doped thin-diameter core rod of the fused support rod processed in step 3 from the left side of the quartz reaction tube into the center of the quartz reaction tube, and fix the support rod on the support tube and tail tube on the MCVD lathe to keep synchronous rotation; Step 5, raising the temperature of the hydrogen-oxygen flame again, setting the pressure in the quartz reaction tube to a negative value, shrinking the quartz reaction tube and the rare earth-doped thin-diameter core rod together into a solid preform, thereby preparing a rare earth-doped optical fiber preform with a large core-to-wrapper ratio.
2. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: The rare earth chelate described in step 1 is heated to a set temperature of 110° C. to 240° C.
3. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: In step 1, the number of deposited core layers is set to 15-20, forming a core-to-shell ratio of 1:
3.
4. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: The rare earth-doped thin-diameter core rod in step 2 is 360 mm in length, and the rare earth-doped thin-diameter core rod is subjected to high-temperature polishing treatment.
5. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: In step 2, the rare earth-doped core in the middle of the rare earth-doped optical fiber preform is drilled and removed as a whole, with the center position of the rare earth-doped core in the middle of the rare earth-doped optical fiber preform as the center of the circle, and a drill bit with a size equal to the diameter of the rare earth-doped core is used to remove it.
6. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: In step 4, the number of deposited core layers is set to 20-30 layers.
7. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: In step 4, the inner diameter of the quartz reaction tube is reduced to 2mm-3mm, which is larger than the diameter of the rare earth-doped thin-diameter core rod.
8. The method for preparing a rare earth-doped optical fiber preform with a large core-to-clad ratio according to claim 1, characterized in that: The rare earth-doped optical fiber preform with a large core-to-clad ratio in step 5 has a core-to-clad ratio of 21:25 or 10:11.
Citation Information
Patent Citations
Method for manufacturing rare earth element-doped optical fiber preform
CN102108008A
Near single module quasi gradient refractive rate large mode field gain optical fiber and preparation method
CN102621626A
Active passive integrated fiber and preparation method thereof
CN108254827A