Preparation of solid waste-based autoclaved aerated concrete board
Thermal expansion cracks and compression resistance of autoclaved aerated concrete slabs were solved by modifying basalt fiber and copper tailings, combined with 2-phosphonobutane-1,2,4-tricarboxylic acid and ammonium dodecyl sulfate Strength issues improve the overall performance of solid waste-based autoclaved aerated concrete panels.
Patent Information
- Application Number
- CN202310320459.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-29
AI Technical Summary
The autoclaved aerated concrete slab causes cracks due to the difference in thermal expansion coefficient after the hydration reaction. In addition, when tailings are used as aggregates, insufficient silicon content and heavy metal ions affect the compressive strength and are not ideal, affecting its application.
Modified basalt fiber and modified copper tailings are used, and through specific processes, such as ultrasonic cleaning, drying, modified liquid impregnation and high-temperature furnace calcination, the properties of the fiber and tailings are improved; 2-phosphine is added to the concrete Acid butane-1,2,4-tricarboxylic acid and ammonium dodecyl sulfate to control the hydration reaction and absorb the heat of hydration.
It significantly improves the crack resistance and compressive strength of the solid waste-based autoclaved aerated concrete slab, reduces the severity of the hydration reaction, and improves the uniformity of the pore structure and thermal performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to preparation of a solid waste-based autoclaved aerated concrete board, belonging to the technical field of concrete preparation. Background Art
[0002] Autoclaved aerated concrete board is a new type of green and environmentally friendly building material with light weight, porous material and cement, lime, silica sand and other materials as the main raw materials. Different amounts of anti-corrosion treated steel mesh are added according to the structural requirements. The autoclaved aerated concrete board with porous crystals is made by batching, mixing, injection molding, pre-curing, cutting and curing under high temperature and high pressure conditions. Its density is lower than that of general cementitious materials, and it has excellent fire resistance, fire prevention, sound insulation, heat insulation, thermal insulation and other unparalleled properties.
[0003] Compared with autoclaved aerated concrete blocks, autoclaved aerated concrete panels need to use built-in steel mesh to solve the problem of poor flexural performance of the panels. However, since the thermal expansion coefficient of general steel is 1.2*10 -5 The thermal expansion coefficient of autoclaved aerated concrete is generally only 0.8*10 -5 When concrete undergoes hydration reaction, a large amount of hydration heat is released, which causes thermal expansion of concrete and steel bars. Different thermal expansion coefficients lead to volume difference between concrete and steel after the hydration reaction is completed, which causes cracks in the concrete slab and affects the performance and use of the autoclaved aerated concrete slab.
[0004] At present, there is also a process of using tailings as concrete aggregate in the raw materials for preparing steam-pressurized concrete. However, the silicon content in the tailings is lower than that in the commonly used river sand and machine-made sand, and it contains heavy metal ions and other impurities, which affect the hydration reaction during the concrete mixing process, resulting in the prepared autoclaved aerated concrete board having unsatisfactory compressive strength performance, thereby affecting the application of the autoclaved aerated concrete board.
[0005] Therefore, a method for preparing an autoclaved aerated concrete slab with good crack resistance and high compressive strength using tailings as aggregate is needed. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a solid waste-based autoclaved aerated concrete board.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention comprises the following steps:
[0008] A solid waste-based autoclaved aerated concrete board, comprising the following components:
[0009] 30-40 parts of cement, 25-35 parts of quicklime, 6-8 parts of desulfurized gypsum, 1-2 parts of aluminum powder, 2-4 parts of modified basalt fiber, 35-45 parts of modified copper tailings, 8-10 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid, and 7-9 parts of ammonium dodecyl sulfate.
[0010] The modified basalt fiber preparation method is:
[0011] (1) 10 parts of basalt fibers were immersed in anhydrous ethanol, and were fully cleaned in an ultrasonic cleaner for 1-2 hours, and then washed twice with deionized water. After washing, the basalt fibers were placed in an oven at 100-110°C and dried to obtain solid a;
[0012] (2) Add 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane to 95% ethanol solution to prepare a solution with a mass fraction of 4% to 6%, thereby obtaining modified solution a. Then, immerse solid a in the modified solution, and heat the system to 35 to 45°C. After keeping the temperature for 6 to 8 hours, take out the solid and wash it with deionized water for 3 times. Then, dry it in an oven at 100 to 110°C to obtain solid b.
[0013] (3) Sodium perfluorononenyloxybenzenesulfonate is dissolved in water to prepare a solution with a mass fraction of 10-12% to obtain the modified liquid b, and then the solid b is immersed in the modified liquid b, and the system is heated to 50-60°C and kept immersed for 25-35 minutes. After the immersion, it is placed in an oven at 100-110°C for drying. After three cycles, the modified basalt fiber is obtained.
[0014] The modified copper tailings preparation method is:
[0015] (1) After 50 parts of copper tailings are ball-milled for 1-2 hours, they are mixed with 10% dilute hydrochloric acid at a mass ratio of 1.8-2:1, and 20%-24% of the mass of copper tailings nitrilotriacetate is added thereto. At the same time, the temperature is raised to 50-56°C at a rate of 3-5°C / min, and the reaction is stirred at a constant temperature for 1-2 hours. After the reaction is completed, the solid a is filtered and the filter residue is washed with deionized water to obtain a solid a and a filtrate a;
[0016] (2) Solid a and 40% sodium hydroxide solution by mass fraction were mixed in a mass ratio of 3:11-13, and reacted at 40-50°C for 1.5-2.5 hours. Then, anhydrous ethanol with a volume of 30% of the sodium hydroxide solution was added to the system, and stirred for 5-10 minutes to make the system uniformly dispersed. Then, 0.1-0.2 mol / L ammonium sulfate solution was added dropwise at a rate of 3-5 drops / s until no precipitation was generated in the system. Then, the mixture was kept warm and reacted at a speed of 35-45 r / min for 4-6 hours. After the reaction was completed, solid b was obtained by filtration.
[0017] (3) Add twice the mass of 20% sodium hydroxide solution to the filtrate a, stir and react for 15-25 min. After the reaction is completed, filter to obtain solid c and filtrate b. Then, pass carbon dioxide gas into the filtrate b until no precipitation is produced. Continue filtering to obtain solid d.
[0018] (4) Solid b and solid d are mixed in a mass ratio of 8-9:1 and placed in a high-temperature furnace for calcination. The mixture is first heated to 250°C at a rate of 3-5°C / min and kept at this temperature for 3-4 hours. The mixture is then heated to 570°C at a rate of 3-5°C / min and kept at this temperature for 1-2 hours. The mixture is finally cooled to room temperature along with the furnace to obtain the modified copper tailings.
[0019] A preparation method of a solid waste-based autoclaved aerated concrete board, the specific process steps are:
[0020] (1) Add cement, quicklime, desulfurized gypsum, modified copper tailings and modified basalt fiber into a mixer and stir evenly for 10 to 20 minutes;
[0021] (2) Mix 2-phosphonobutane-1,2,4-tricarboxylic acid and 20-24 parts of water and add to a blender and continue to stir for 3-5 minutes;
[0022] (3) Mix aluminum powder and water in a mass ratio of 1:10-20 and add to a blender. Continue stirring for 1-2 minutes.
[0023] (4) Add ammonium dodecyl sulfate into the mixer while stirring for about 30 to 60 seconds, and continue stirring for 1 to 2 minutes after the addition is completed to obtain a concrete slab slurry;
[0024] (5) The concrete slab slurry is poured into the module, and then sent to a curing room at a temperature of 55-65°C for pre-curing for 3-4 hours to obtain an aerated concrete slab body. After removing the mold, the aerated concrete slab is cut into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0025] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1~-0.05MPa, then introduce steam to increase the pressure to 1.4~1.8MPa at a rate of 0.04~0.06MPa / min, and increase the temperature to 180℃~200℃ at a rate of 1~3℃ / min, then maintain constant temperature and pressure for 7.5~8.5h, finally stop introducing steam and reduce the pressure to normal pressure within 30~40min, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board.
[0026] The beneficial effects of the present invention are:
[0027] (1) Sodium perfluorononenyloxybenzene sulfonate has excellent surface properties and can significantly reduce the surface tension of basalt fiber, making it easier to wet. It can also eliminate the surface charge of basalt and reduce the agglomeration of basalt fiber. Its sulfonate group can also promote the hydration reaction of concrete and reduce the molding time of concrete. The large number of fluorine groups in sodium perfluorononenyloxybenzene sulfonate can improve the flame retardancy of concrete.
[0028] (2) 3-[Bis(2-hydroxyethyl)amino]propane-triethoxysilane is a silane coupling agent that can form a large number of stable silicon-oxygen bonds on the surface of basalt fiber, thereby improving the surface properties of basalt fiber and enhancing the wetting and dispersion properties of basalt fiber. It also contains two hydrophilic hydroxyl groups, which can also enhance the wetting properties of basalt fiber. The surface roughness of basalt fiber is also significantly improved after modification, which is conducive to better wetting of sodium perfluorononenyloxybenzenesulfonate on the basalt surface during modification.
[0029] (3) Nitrilotriacetate can complex the heavy metal ions precipitated from the copper tailings. On the one hand, it can accelerate the precipitation of heavy metal ions, and on the other hand, it can make the precipitation amount of heavy metal ions greater. Nitrilotriacetate is not resistant to concentrated alkali, which makes it convenient to dissociate the complexed aluminum ions by adding strong alkali to use as the raw material for recovering aluminum dioxide. Nitrilotriacetate trisalt is easily biodegradable and environmentally friendly.
[0030] (4) Ammonium sulfate solution is weaker in acidity than strong acid, so the reaction with sodium silicate is not so violent, so the particle size distribution of the generated silicate precipitate will not be too different. In addition, the sodium sulfate generated after the reaction can also be used as an accelerator when mixing concrete, without the introduction of other impurities.
[0031] (5) After adding ammonium sulfate, continue the reaction for 4 to 6 hours so that the generated silica precipitates can attract each other and aggregate into micron-sized particles, avoiding poor concrete mixing effect due to self-agglomeration when added to the concrete system after calcination into nano-silicon dioxide, thus affecting various properties of the concrete;
[0032] (6) After modification, basalt fiber has excellent dispersibility and wettability, which can enhance the fluidity of concrete, thereby increasing the reaction area between cement particles and water and promoting the hydration reaction. The sulfonate in sodium perfluorononenyloxybenzenesulfonate can also promote the hydration reaction process. After the copper tailings are processed, the silicon content can be increased and the reaction activity of silica can be improved, which can also promote the hydration reaction. However, too fast a hydration reaction will lead to the release of too much heat, thereby affecting the gas production process of the air entraining agent, making the pore structure uneven, the pore size too large and the number of irregular pores increased, thereby reducing the thermal performance of autoclaved aerated concrete. 2-Phosphonobutane-1,2,4-tricarboxylic acid is a hydroxycarboxylic acid complex. The hydrogen ions it contains first react with the hydroxide in the concrete to reduce the hydroxide ion concentration in the concrete, and then they can react with Ca 2+ Formation of unstable complexes that can control Ca in the early stages of hydration 2+ The concentration of these two steps can inhibit the hydration reaction, thereby reducing the intensity of the hydration reaction and reducing the heat generation;
[0033] (7) Ammonium dodecyl sulfate is an ammonium salt. It absorbs heat when dissolved in water, thereby absorbing part of the heat of hydration. It also has foaming properties, which can assist in the generation of bubbles and act as an air entraining agent. Implementation
[0034] The present invention will be further described in detail below in conjunction with the embodiments. Example 1
[0035] 10 parts of basalt fiber were immersed in anhydrous ethanol, and fully cleaned in an ultrasonic cleaner for 1.5 hours, and then washed twice with deionized water. After washing, the basalt fiber was placed in a 105°C oven to dry to obtain solid a. 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane was added to a 95% ethanol solution to prepare a 5% mass fraction solution to obtain a modified liquid a. Then, solid a was immersed in the modified liquid, and the system was heated to 40°C. After insulation reaction for 7 hours, it was taken out and washed three times with deionized water, and placed in a 105°C oven to dry to obtain solid b. Sodium perfluorononenyloxybenzenesulfonate was dissolved in water to prepare a solution with a mass fraction of 11%, to obtain a modified liquid b. Then, solid b was immersed in the modified liquid b, and the system was heated to 55°C for insulation and immersion for 30 minutes. After immersion, it was placed in a 105°C oven to dry. After three cycles, the modified basalt fiber was obtained.
[0036] After ball milling 50 parts of copper tailings for 1.5 hours, they were mixed with 10% dilute hydrochloric acid at a mass ratio of 1.9:1, and 22% of the mass of copper tailings was added thereto. At the same time, the temperature was raised to 53°C at a rate of 4°C / min, and the reaction was stirred at a constant temperature for 1.5 hours. After the reaction, it was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a. Solid a and 40% mass fraction sodium hydroxide solution were mixed at a mass ratio of 1:4, and reacted at 45°C for 2 hours. Then, 30% of the volume of sodium hydroxide solution in anhydrous ethanol was added to the system, and the system was stirred for 8 minutes to make the system uniformly dispersed. Then, 0.15 mol / L ammonium sulfate solution was added dropwise at a rate of 4 drops / s until no more precipitation was produced in the system. Then keep warm and continue to react at a speed of 40r / min for 5h. After the reaction is completed, filter to obtain solid b; add twice the mass of 20% mass fraction sodium hydroxide solution to the filtrate a, stir and react for 20min, filter to obtain solid c and filtrate b after the reaction is completed, then pass carbon dioxide gas into the filtrate b until no more precipitation is produced, and continue to filter to obtain solid d; mix solid b and solid d in a mass ratio of 8.5:1 and put them into a high-temperature furnace for calcination, first increase the temperature to 250℃ at a speed of 4℃ / min, keep the temperature constant for 3.5h, then continue to increase the temperature to 570℃ at a speed of 4℃ / min, keep the temperature constant for 1.5h, and finally cool to room temperature with the furnace to obtain modified copper tailings.
[0037] (1) Add 35 parts of cement, 30 parts of quicklime, 7 parts of desulfurized gypsum and 40 parts of modified copper tailings into a mixer and stir evenly for 15 minutes;
[0038] (2) Mix 9 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid and 22 parts of water and add to a blender and continue to stir for 4 minutes;
[0039] (3) Mix 1.5 parts of aluminum powder and water in a mass ratio of 1:15 and add them into a blender. Continue stirring for 1.5 minutes.
[0040] (4) Add 8 parts of ammonium dodecyl sulfate into the mixer while stirring over a period of about 45 seconds. Continue stirring for 1.5 minutes after the addition is complete to obtain a concrete slab slurry.
[0041] (5) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 60°C for pre-curing for 3.5 hours to obtain an aerated concrete slab blank, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0042] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.07 MPa, then introduce steam to increase the pressure to 1.6 MPa at a rate of 0.05 MPa / min, and increase the temperature to 190°C at a rate of 2°C / min, then maintain constant temperature and pressure for 8 hours, finally stop introducing steam and reduce the pressure to normal pressure within 35 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board. Example 2
[0043] 10 parts of basalt fiber were immersed in anhydrous ethanol, and fully cleaned in an ultrasonic cleaner for 1 hour, and then washed twice with deionized water. After washing, the basalt fiber was placed in a 110°C oven to dry to obtain solid a; 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane was added to a 95% ethanol solution to prepare a 6% mass fraction solution to obtain a modified liquid a, and then solid a was immersed in the modified liquid, and the system was heated to 35°C. After insulation reaction for 8 hours, it was taken out and washed three times with deionized water, and then placed in a 100°C oven to dry to obtain solid b; sodium perfluorononenyloxybenzenesulfonate was dissolved in water to prepare a 12% mass fraction solution to obtain a modified liquid b, and then solid b was immersed in the modified liquid b, and the system was heated to 50°C and impregnated for 35 minutes. After impregnation, it was placed in a 110°C oven to dry, and after three cycles, the modified basalt fiber was obtained.
[0044] After 50 parts of copper tailings were ball-milled for 2 hours, they were mixed with 10% dilute hydrochloric acid at a mass ratio of 1.8:1, and 20% of the mass of copper tailings was added thereto. At the same time, the temperature was raised to 56°C at a rate of 3°C / min, and the reaction was stirred at a constant temperature for 1 hour. After the reaction was completed, it was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a. Solid a and 40% mass fraction sodium hydroxide solution were mixed at a mass ratio of 3:11, and reacted at 40°C for 2.5 hours. Then, 30% of the volume of sodium hydroxide solution was added to the system. Anhydrous ethanol was stirred for 5 minutes to make the system evenly dispersed, and then 0.2 mol / L ammonium sulfate solution was added at a rate of 3 drops / s until no precipitation was generated in the system. , then keep warm and continue to react at a speed of 45r / min for 4h. After the reaction is completed, filter to obtain solid b, add twice the mass of 20% mass fraction sodium hydroxide solution to the filtrate a, stir and react for 15min, filter to obtain solid c and filtrate b after the reaction is completed, then pass carbon dioxide gas into the filtrate b until no more precipitation is produced, continue to filter to obtain solid d, mix solid b and solid d in a mass ratio of 8:1 and put them into a high-temperature furnace for calcination, first heat to 250℃ at a speed of 3℃ / min, keep the temperature for 4h, then continue to heat to 570℃ at a speed of 5℃ / min, keep the temperature for 1h, and finally cool to room temperature with the furnace to obtain modified copper tailings.
[0045] (1) Add 30 parts of cement, 35 parts of quicklime, 8 parts of desulfurized gypsum, 35 parts of modified copper tailings and 2 parts of modified basalt fiber into a mixer and stir evenly for 10 minutes;
[0046] (2) Mix 8 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid and 20 parts of water and add them into a blender and continue to stir for 3 minutes;
[0047] (3) Mix 2 parts of aluminum powder and water in a mass ratio of 1:20 and add into a blender, and continue to stir for 2 minutes;
[0048] (4) Add 9 parts of ammonium dodecyl sulfate into the mixer while stirring over a period of about 30 seconds. Continue stirring for 2 minutes after the addition is complete to obtain a concrete slab slurry.
[0049] (5) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 65°C for pre-curing for 3 hours to obtain an aerated concrete slab blank, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0050] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.05 MPa, then introduce steam to increase the pressure to 1.8 MPa at a rate of 0.04 MPa / min, and increase the temperature to 180°C at a rate of 3°C / min, then maintain constant temperature and pressure for 7.5 hours, finally stop introducing steam and reduce the pressure to normal pressure within 40 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board. Example 3
[0051] 10 parts of basalt fiber were immersed in anhydrous ethanol, and fully cleaned in an ultrasonic cleaner for 2 hours, and then washed twice with deionized water. After washing, the basalt fiber was placed in a 100°C oven to dry to obtain solid a; 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane was added to a 95% ethanol solution to prepare a 4% mass fraction solution to obtain a modified liquid a, and then solid a was immersed in the modified liquid, and the system was heated to 45°C. After keeping warm for 6 hours, it was taken out and washed three times with deionized water, and then placed in a 110°C oven to dry to obtain solid b; sodium perfluorononenyloxybenzenesulfonate was dissolved in water to prepare a 10% mass fraction solution to obtain a modified liquid b, and then solid b was immersed in the modified liquid b, and the system was heated to 60°C and kept warm for 25 minutes. After impregnation, it was placed in a 100°C oven to dry, and after three cycles, the modified basalt fiber was obtained.
[0052] After ball milling for 1 hour, 50 parts of copper tailings were mixed with 10% dilute hydrochloric acid at a mass ratio of 2:1, and 24% of the mass of copper tailings nitrilotriacetate was added thereto. At the same time, the temperature was raised to 50°C at a rate of 5°C / min, and the reaction was stirred at a constant temperature for 2 hours. After the reaction was completed, the solid a was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a; solid a and 40% mass fraction sodium hydroxide solution were mixed at a ratio of 3: 13 by mass ratio, react at 50 ℃ for 1.5h, then add anhydrous ethanol with a volume of 30% of the sodium hydroxide solution to the system, stir for 10min to make the system uniformly dispersed, then add 0.1mol / L ammonium sulfate solution at a rate of 3 drops / s until no precipitation is generated in the system, then keep warm and continue to react at a speed of 35r / min for 6h, filter to obtain solid b after the reaction is completed; add 20% mass fraction sodium hydroxide solution twice its mass to the filtrate a, stir and react for 15min, filter to obtain solid c and filtrate b after the reaction is completed, then pass carbon dioxide gas into the filtrate b until no precipitation is generated, and continue to filter to obtain solid d; solid b and solid d are mixed in a mass ratio of 9:1 and put into a high-temperature furnace together for calcination, first heat to 250 ℃ at a rate of 5 ℃ / min, keep constant temperature for 3h, then continue to heat to 570 ℃ at a rate of 3 ℃ / min, keep constant temperature for 2h, and finally cool to room temperature with the furnace to obtain modified copper tailings.
[0053] (1) Add 40 parts of cement, 25 parts of quicklime, 6 parts of desulfurized gypsum and 45 parts of modified copper tailings into a mixer and stir evenly for 20 minutes;
[0054] (2) Mix 10 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid and 24 parts of water and add them into a blender and continue to stir for 5 minutes;
[0055] (3) Mix 1 part aluminum powder and water in a mass ratio of 1:10 and add into a blender, and continue to stir for 1 minute;
[0056] (4) Add 7 parts of ammonium dodecyl sulfate into the mixer while stirring for about 60 seconds, and continue stirring for 1 minute after the addition is completed to obtain a concrete slab slurry;
[0057] (5) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 55°C for pre-curing for 4 hours to obtain an aerated concrete slab body, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0058] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1 MPa, then introduce steam to increase the pressure to 1.4 MPa at a rate of 0.06 MPa / min, and increase the temperature to 200°C at a rate of 1°C / min, then maintain constant temperature and pressure for 8.5 hours, finally stop introducing steam and reduce the pressure to normal pressure within 30 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board. Example 4
[0059] Preparation method of modified basalt fiber:
[0060] 10 parts of basalt fiber were immersed in anhydrous ethanol and thoroughly cleaned in an ultrasonic cleaner for 1.5 hours, then washed twice with deionized water, and after washing, the basalt fiber was placed in a 105°C oven to dry to obtain solid a, sodium perfluorononenyloxybenzenesulfonate was dissolved in water to prepare a solution with a mass fraction of 11%, and then the modified liquid a was obtained, and then the solid a was immersed in the modified liquid a, and the system was heated to 55°C and kept immersed for 30 minutes. After the impregnation, it was placed in a 105°C oven to dry, and the modified basalt fiber was obtained after three cycles.
[0061] The rest is the same as in Example 1. Example 5
[0062] Preparation method of modified basalt fiber:
[0063] Ten parts of basalt fibers were immersed in anhydrous ethanol and thoroughly cleaned in an ultrasonic cleaner for 1.5 hours, then washed twice with deionized water, and after washing, the basalt fibers were placed in a 105°C oven to dry to obtain solid a, 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane was added to a 95% ethanol solution to prepare a 5% mass fraction solution to obtain a modified liquid a, and then solid a was immersed in the modified liquid, and the system was heated to 40°C. After the reaction was kept warm for 7 hours, it was taken out and washed three times with deionized water, and then placed in a 105°C oven to dry to obtain the modified basalt fiber.
[0064] The rest is the same as in Example 1. Example 6
[0065] Modified basalt fiber preparation method:
[0066] 10 parts of basalt fiber were added to anhydrous ethanol, and fully cleaned in an ultrasonic cleaner for 1.5 hours, and then washed twice with deionized water. After washing, the basalt fiber was placed in a 105°C oven to dry to obtain solid a. Vinyl triethoxysilane was added to a 95% ethanol solution, and then acetic acid was added to adjust the pH to 5.0 and then configured into a 5% mass fraction solution to obtain a modified liquid a. Then solid a was added to the modified liquid, and the system was heated to 40°C. After insulation reaction for 7 hours, it was taken out and washed with deionized water for 3 times, and then placed in a 105°C oven to dry to obtain solid b. Polyethylene glycol was dissolved in water to prepare a solution with a mass fraction of 11%, that is, to obtain a modified liquid b. Then solid b was added to the modified liquid b, and the system was heated to 55°C and impregnated for 30 minutes. After impregnation, it was placed in a 105°C oven to dry. After 3 cycles, the modified basalt fiber was obtained.
[0067] The rest is the same as in Example 1. Example 7
[0068] The difference between this embodiment and embodiment 1 is that the 95% ethanol solution is replaced by deionized water. Example 8
[0069] Preparation method of modified copper tailings:
[0070] After ball milling for 2 hours, 50 parts of copper tailings were mixed with 10% dilute hydrochloric acid at a mass ratio of 1.8:1, and the temperature was raised to 56°C at a rate of 3°C / min. The reaction was stirred at a constant temperature for 1 hour. After the reaction was completed, it was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a. Solid a and 40% mass fraction sodium hydroxide solution were mixed at a mass ratio of 3:11, and reacted at 40°C for 2.5 hours. Then, 30% of the volume of sodium hydroxide solution was added to the system. Anhydrous ethanol was stirred for 5 minutes to make the system uniformly dispersed, and then 0.2 mol / L ammonium sulfate solution was added at a rate of 3 drops / s until no precipitation was generated in the system. Then, the temperature was kept and heated at 45r / m in, and continue to react for 4 hours. After the reaction is completed, filter to obtain solid b. Add twice the mass of 20% mass fraction sodium hydroxide solution to the filtrate a, stir and react for 15 minutes. After the reaction is completed, filter to obtain solid c and filtrate b. Then, introduce carbon dioxide gas into the filtrate b until no more precipitation is produced. Continue to filter to obtain solid d. Mix solid b and solid d in a mass ratio of 8:1 and put them into a high-temperature furnace for calcination. First, heat to 250°C at a rate of 3°C / min and keep the temperature constant for 4 hours. Then, continue to heat to 570°C at a rate of 5°C / min and keep the temperature constant for 1 hour. Finally, cool to room temperature with the furnace to obtain modified copper tailings.
[0071] The rest is the same as Example 2. Example 9
[0072] The difference between this embodiment and embodiment 2 is that the 0.2 mol / L ammonium sulfate solution is replaced by a 0.2 mol / L dilute hydrochloric acid solution. Example 10
[0073] Preparation method of modified copper tailings:
[0074] After 50 parts of copper tailings were ball-milled for 2 hours, they were mixed with 10% dilute hydrochloric acid at a mass ratio of 1.8:1, and 20% of the mass of copper tailings was added to the mixture. At the same time, the temperature was raised to 56°C at a rate of 3°C / min, and the reaction was stirred at a constant temperature for 1 hour. After the reaction was completed, it was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a. Solid a and 40% mass fraction sodium hydroxide solution were mixed at a mass ratio of 3:11, and reacted at 40°C for 2.5 hours. Then, 30% of the volume of sodium hydroxide solution was added to the system. Anhydrous ethanol was stirred for 5 minutes to make the system evenly dispersed, and then 0.2 mol / L ammonium sulfate was added at a rate of 3 drops / s. Solution, until no more precipitation is produced in the system, filter to obtain solid b, add twice the mass of 20% mass fraction sodium hydroxide solution to the filtrate a, stir and react for 15 minutes, after the reaction is completed, filter to obtain solid c and filtrate b, then pass carbon dioxide gas into the filtrate b until no more precipitation is produced, continue to filter to obtain solid d, mix solid b and solid d in a mass ratio of 8:1, and put them into a high-temperature furnace for calcination, first raise the temperature to 250°C at a rate of 3°C / min, keep the temperature for 4h, then continue to raise the temperature to 570°C at a rate of 5°C / min, keep the temperature for 1h, and finally cool to room temperature with the furnace to obtain modified copper tailings.
[0075] The rest is the same as Example 2. Embodiment 11
[0076] Preparation method of modified copper tailings:
[0077] After 50 parts of copper tailings were ball-milled for 2 hours, they were mixed with 10% dilute hydrochloric acid at a mass ratio of 1.8:1, and 20% of the mass of copper tailings was added to the mixture. At the same time, the temperature was raised to 56°C at a rate of 3°C / min, and the reaction was stirred at a constant temperature for 1 hour. After the reaction was completed, it was filtered and the filter residue was washed with deionized water to obtain solid a and filtrate a. Solid a and 40% mass fraction sodium hydroxide solution were mixed at a mass ratio of 3:11, and reacted at 40°C for 2.5 hours. Then, 30% of the volume of sodium hydroxide solution was added to the system. Anhydrous ethanol was stirred for 5 minutes to make the system evenly dispersed, and then 0.2 mol / L ammonium sulfate was added at a rate of 3 drops / s. The solution was added until no precipitation was produced in the system, and then the temperature was kept and the reaction was continued at a speed of 45r / min for 4h. After the reaction was completed, solid b was obtained by filtering, and twice the mass of 20% mass fraction sodium hydroxide solution was added to the filtrate a, and the reaction was stirred for 15min. After the reaction was completed, solid c and filtrate b were obtained by filtering, and then carbon dioxide gas was introduced into the filtrate b until no precipitation was produced, and solid d was obtained by continuing to filter. Solid b and solid d were mixed in a mass ratio of 8:1, and then put into a high-temperature furnace together for calcination, and the temperature was raised to 570℃ at a rate of 5℃ / min, kept constant for 1h, and finally cooled to room temperature with the furnace to obtain modified copper tailings.
[0078] The rest is the same as Example 2. Example 12
[0079] Preparation method of solid waste based autoclaved aerated concrete board:
[0080] (1) Add 40 parts of cement, 25 parts of quicklime, 6 parts of desulfurized gypsum and 45 parts of modified copper tailings into a mixer and stir evenly for 20 minutes;
[0081] (2) Add 24 parts of water into the blender and continue blending for 5 minutes;
[0082] (3) Mix 1 part aluminum powder and water in a mass ratio of 1:10 and add into a blender, and continue to stir for 1 minute;
[0083] (4) Add 7 parts of ammonium dodecyl sulfate into the mixer while stirring for about 60 seconds, and continue stirring for 1 minute after the addition is completed to obtain a concrete slab slurry;
[0084] (5) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 55°C for pre-curing for 4 hours to obtain an aerated concrete slab body, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0085] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1 MPa, then introduce steam to increase the pressure to 1.4 MPa at a rate of 0.06 MPa / min, and increase the temperature to 200°C at a rate of 1°C / min, then maintain constant temperature and pressure for 8.5 hours, finally stop introducing steam and reduce the pressure to normal pressure within 30 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board.
[0086] The rest is the same as in Example 3. Example 13
[0087] Preparation method of solid waste based autoclaved aerated concrete board:
[0088] (1) Add 40 parts of cement, 25 parts of quicklime, 6 parts of desulfurized gypsum and 45 parts of modified copper tailings into a mixer and stir evenly for 20 minutes;
[0089] (2) Mix 10 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid and 24 parts of water and add them into a blender and continue to stir for 5 minutes;
[0090] (3) Mix 1 part aluminum powder and water in a mass ratio of 1:10 and add into a blender, and continue to stir for 1 minute;
[0091] (4) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 55°C for pre-curing for 4 hours to obtain an aerated concrete slab body, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0092] (5) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1 MPa, then introduce steam to increase the pressure to 1.4 MPa at a rate of 0.06 MPa / min, and increase the temperature to 200°C at a rate of 1°C / min, then maintain constant temperature and pressure for 8.5 hours, finally stop introducing steam and reduce the pressure to normal pressure within 30 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board.
[0093] The rest is the same as in Example 3. Embodiment 14
[0094] Preparation method of solid waste based autoclaved aerated concrete board:
[0095] (1) Add 40 parts of cement, 25 parts of quicklime, 6 parts of desulfurized gypsum and 45 parts of modified copper tailings into a mixer and stir evenly for 20 minutes;
[0096] (2) Mix 10 parts of 2-phosphonobutane-1,2,4-tricarboxylic acid and 24 parts of water and add them into a blender and continue to stir for 5 minutes;
[0097] (3) Mix 1 part aluminum powder and water in a mass ratio of 1:10 and add into a blender, and continue to stir for 1 minute;
[0098] (4) Add 7 parts of ammonium dodecyl sulfate into the mixer at one time and continue stirring for 1 minute to obtain a concrete slab slurry;
[0099] (5) pouring the concrete slab slurry into the module, and then sending it into a curing room at a temperature of 55°C for pre-curing for 4 hours to obtain an aerated concrete slab body, and after removing the mold, cutting it into the required size to obtain a formed solid waste-based steam-pressurized concrete slab;
[0100] (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1 MPa, then introduce steam to increase the pressure to 1.4 MPa at a rate of 0.06 MPa / min, and increase the temperature to 200°C at a rate of 1°C / min, then maintain constant temperature and pressure for 8.5 hours, finally stop introducing steam and reduce the pressure to normal pressure within 30 minutes, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board.
[0101] The rest is the same as in Example 3.
[0102] The solid waste-based autoclaved aerated concrete slab formed in the example was tested for surface cracks and evaluated according to the evaluation criteria in Table 1.
[0103]
[0104] The compressive strength and thermal conductivity of the autoclaved aerated concrete board prepared in the embodiment were tested according to the provisions of GB / T15762-2020 and GB / T11968-2020.
[0105] Some process technology features and technical indicators of Examples 1, 2 and 3 of the present invention are compared, as shown in Table 2.
[0106]
[0107] The process technology features and technical indicators of Example 1 of the present invention are compared with those of Examples 4 to 7, as shown in Table 3.
[0108]
[0109] The process technology features and technical indicators of Example 2 of the present invention are compared with those of Examples 8 to 11, as shown in Table 4.
[0110]
[0111] Some process technology features and technical indicators of Example 3 of the present invention are compared with those of Examples 12, 13, and 14, as shown in Table 5.
[0112]
[0113] Combining the data in Tables 2, 3, 4 and 5, it can be seen that the present invention significantly improves the crack resistance of the solid waste-based autoclaved aerated concrete board by adding basalt fiber to the components of the solid waste-based autoclaved aerated concrete board. Since the basalt fiber has poor dispersibility in concrete, after modification, the solid waste-based autoclaved aerated concrete board has no cracks on the surface and is intact as a whole. By modifying the copper tailings, the problem of substandard compressive strength of the solid waste-based autoclaved aerated concrete board caused by low silicon content, large particle size and heavy metal ions in the copper tailings is solved. The initial hydration reaction caused by the maintenance and modification of copper tailings is too violent, releasing too much heat, affecting the gas production process of the air-entraining agent in the concrete, making the internal pore structure of the solid waste-based autoclaved aerated concrete board uneven, the pore size too large and the number of irregular pores increased, thereby reducing the thermal performance of the solid waste-based autoclaved aerated concrete board. By adding 2-phosphonobutane-1,2,4-tricarboxylic acid and ammonium dodecyl sulfate to the components of the solid waste-based autoclaved aerated concrete board, the hydration reaction is inhibited and part of the hydration heat is absorbed, thereby reducing the negative effects of excessive hydration heat.
Claims
1. A method for preparing a solid waste-based autoclaved aerated concrete board, characterized in that: The specific process steps are: (1) Add 30-40 parts by weight of cement, 25-35 parts by weight of quicklime, 6-8 parts by weight of desulfurized gypsum, 35-45 parts by weight of modified copper tailings and 2-4 parts by weight of modified basalt fiber into a mixer and stir evenly for 10-20 minutes; (2) Mix 8 to 10 parts by weight of 2-phosphonobutane-1,2,4-tricarboxylic acid and 20 to 24 parts of water and add the mixture into a blender and continue to blend for 3 to 5 minutes; (3) Mix 1-2 parts by weight of aluminum powder and water in a mass ratio of 1:10-20 and add to a blender, and continue to stir for 1-2 minutes; (4) adding 7 to 9 parts by weight of ammonium dodecyl sulfate into a mixer while stirring for about 30 to 60 seconds, and continuing to stir for 1 to 2 minutes after the addition is completed to obtain a concrete slab slurry; (5) The concrete slab slurry is poured into the module, and then sent to a curing room at a temperature of 55-65°C for pre-curing for 3-4 hours to obtain an aerated concrete slab body. After removing the mold, the aerated concrete slab is cut into the required size to obtain a formed solid waste-based steam-pressurized concrete slab; (6) Place the formed solid waste-based steam-pressurized concrete board into an autoclave, first evacuate the autoclave to -0.1~-0.05MPa, then introduce steam to increase the pressure to 1.4~1.8MPa at a rate of 0.04~0.06MPa / min, and increase the temperature to 180℃~200℃ at a rate of 1~3℃ / min, then maintain constant temperature and pressure for 7.5~8.5h, finally stop introducing steam and reduce the pressure to normal pressure within 30~40min, and then naturally cool to room temperature with the autoclave to obtain the finished solid waste-based autoclaved aerated concrete board; Among them, the preparation method of modified basalt fiber is: (1) Immerse the basalt fiber in anhydrous ethanol and fully clean it in an ultrasonic cleaner for 1-2 hours, then wash it twice with deionized water. After washing, put the basalt fiber into an oven at 100-110°C to dry it to obtain solid a; (2) Add 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane to 95% ethanol solution to prepare a solution with a mass fraction of 4% to 6%, thereby obtaining modified solution a. Then, immerse solid a in the modified solution, and heat the system to 35 to 45°C. After keeping the temperature for 6 to 8 hours, take out the solid and wash it with deionized water for 3 times. Then, dry it in an oven at 100 to 110°C to obtain solid b. (3) Sodium perfluorononenyloxybenzenesulfonate is dissolved in water to prepare a solution with a mass fraction of 10-12%, thereby obtaining a modified liquid b, and then solid b is immersed in the modified liquid b, and the system is heated to 50-60°C and kept immersed for 25-35 minutes. After the immersion, the system is placed in an oven at 100-110°C for drying, and the modified basalt fiber is obtained after three cycles; Wherein, the preparation method of modified copper tailings is: (1) After ball milling the copper tailings for 1 to 2 hours, mix it with 10% dilute hydrochloric acid at a mass ratio of 1.8 to 2:1, and add nitrilotriacetate at a mass ratio of 20% to 24% of the mass of the copper tailings. At the same time, heat it to 50 to 56°C at a rate of 3 to 5°C / min, stir it at a constant temperature for 1 to 2 hours, filter it after the reaction, and wash the filter residue with deionized water to obtain solid a and filtrate a; (2) Solid a and 40% sodium hydroxide solution by mass fraction were mixed in a mass ratio of 3:11-13, and reacted at 40-50°C for 1.5-2.5 hours. Then, anhydrous ethanol with a volume of 30% of the sodium hydroxide solution was added to the system, and stirred for 5-10 minutes to make the system uniformly dispersed. Then, 0.1-0.2 mol / L ammonium sulfate solution was added dropwise at a rate of 3-5 drops / s until no precipitation was generated in the system. Then, the mixture was kept warm and reacted at a speed of 35-45 r / min for 4-6 hours. After the reaction was completed, solid b was obtained by filtration. (3) Add twice the mass of 20% sodium hydroxide solution to the filtrate a, stir and react for 15-25 min. After the reaction is completed, filter to obtain solid c and filtrate b. Then, pass carbon dioxide gas into the filtrate b until no precipitation is produced. Continue filtering to obtain solid d. (4) Solid b and solid d are mixed in a mass ratio of 8-9:1 and placed in a high-temperature furnace for calcination. The mixture is first heated to 250°C at a rate of 3-5°C / min and kept at this temperature for 3-4 hours. The mixture is then heated to 570°C at a rate of 3-5°C / min and kept at this temperature for 1-2 hours. The mixture is finally cooled to room temperature along with the furnace to obtain the modified copper tailings.
Citation Information
Patent Citations
Improvements in or relating to maximum safe load indicators for cranes
GB1030104A
Method for continuously extracting scattered metals in tailings by using supercritical CO2
CN114959265A
KR1017914120000B1