Polyurethane coating combination system and its coating products and applications
By using polyisocyanate curing agents with high functionality and high NCO content, the crosslinking network of polyurethane coatings is enhanced, overcoming the shortcomings of traditional coatings in terms of sun protection and scratch resistance, achieving higher hardness, abrasion resistance and chemical resistance, while maintaining good adhesion and appearance.
Patent Information
- Application Number
- CN202111679666.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-12-31
AI Technical Summary
Traditional polyurethane coatings for automotive interiors are insufficient in terms of sun protection and scratch resistance, especially at low gloss levels, where they are difficult to withstand the chemical erosion of high sun protection and are prone to gloss marks.
High-functionality and high-NCO content polyisocyanate is used as a curing agent, which works synergistically with hydroxyl-containing components and additives in the main formulation to increase the crosslinking ability of the coating system, form a tighter crosslinking network, improve the density and hardness of the coating, and enhance wear resistance and chemical resistance.
It improves the hardness, abrasion resistance and chemical resistance of the coating, enabling it to withstand SPF50+++ sunscreen and 100% octyl salicylate, maintain good adhesion to the substrate, and retain a delicate and uniform appearance under low gloss.
Smart Images

Figure QLYQS_1 
Figure BDA0003453646730000021 
Figure BDA0003453646730000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a polyurethane coating combination system and a coating product and application thereof. Background Art
[0002] Automotive interior polyurethane (PU) coatings are mainly used for surface coating of interior parts such as door panels, buttons, and instrument panel sunshades. The glossiness is generally 2° to 5°, with good scratch resistance and a delicate and uniform appearance. The common components of automotive interior PU coatings generally include: resin, pigments, fillers, solvents, additives, and curing agents (the curing agents commonly used in the prior art are low-functionality isocyanates, such as diisocyanates, diisocyanate oligomers, such as Digo T1890E, Covestro Z4470, Covestro N3580BA, Asahi Kasei TKA100, Covestro L75, Covestro The reaction mechanism of N 3390 and Covestro N75 is that -OH (hydroxyl-containing components, such as resin) and -NCO (curing agent) undergo cross-linking reaction and cure to form a coating.
[0003] The chemical resistance of traditional PU coatings, especially the sunscreen resistance, is relatively average. Even through the optimization of resin, curing agent and filler, it is difficult to pass some more stringent sunscreen resistance tests (such as NIVEA SPF30PA++). In addition, the scratch resistance of PU coatings is also poor under low gloss conditions, and it is easy to produce bright marks after scratching with nails. Therefore, it is necessary to further develop PU coatings with improved sunscreen resistance and scratch resistance. Summary of the invention
[0004] Based on this, one of the objects of the present invention is to provide a polyurethane coating combination system that can tolerate SPF50+++ sunscreen cream and 100% octyl salicylate. The polyurethane coating product prepared by the polyurethane coating combination system also has improved hardness and wear resistance and good substrate adhesion.
[0005] The above-mentioned object of the invention can be achieved through the following technical solutions.
[0006] In a first aspect of the present invention, a polyurethane coating system is provided, comprising component A, component B and component C in a weight ratio of 100:(5-30):(70-100):
[0007] The component A comprises a hydroxy acrylic resin, a thermoplastic acrylic resin, a polyester polyol resin and a mixed solvent; wherein the hydroxy value of the hydroxy acrylic resin is 20 to 100 mgKOH / g; the hydroxy value of the polyester polyol resin is 100 to 400 mgKOH / g; the mixed solvent comprises a low boiling point solvent with a boiling point below 100°C and a medium boiling point solvent with a boiling point of 100°C to 120°C;
[0008] The component B is a polyisocyanate curing agent, with an NCO content of ≥25% and an NCO functionality of ≥10;
[0009] The component C is a diluent.
[0010] In some embodiments, in the component A, based on 100 parts by weight, the following are included:
[0011]
[0012] In some embodiments, in the component A, the hydroxy acrylic resin is 30 to 40 parts by weight; and / or,
[0013] The molecular weight of the hydroxy acrylic resin is 20 kDa to 100 kDa; and / or,
[0014] The hydroxy value of the hydroxy acrylic resin is 30 to 80 mgKOH / g; and / or,
[0015] The Tg of the hydroxy acrylic resin is 65° C. to 100° C.; and / or,
[0016] The thermoplastic acrylic resin is 4 to 8 parts by weight; and / or,
[0017] The molecular weight of the thermoplastic acrylic resin is 50 kDa to 200 kDa; and / or;
[0018] The Tg of the thermoplastic acrylic resin is 90° C. to 120° C.; and / or,
[0019] The polyester polyol resin is 3 to 5 parts by weight; and / or,
[0020] The molecular weight of the polyester polyol resin is 500Da to 5000Da; and / or,
[0021] The polyester polyol resin has a hydroxyl value of 100 to 350 mgKOH / g; and / or,
[0022] The low boiling point solvent is 15 to 25 parts by weight; and / or,
[0023] The low boiling point solvent is one or more of ethyl acetate, isopropyl acetate and butanone; and / or,
[0024] The medium boiling point solvent is 10 to 20 parts by weight; and / or,
[0025] The medium boiling point solvent is one or more of n-butyl acetate, isobutyl acetate, sec-butyl acetate and methyl isobutyl ketone.
[0026] In some embodiments, in the component A,
[0027] The molecular weight of the hydroxy acrylic resin is 30 kDa to 80 kDa; and / or,
[0028] The Tg of the hydroxy acrylic resin is 70° C. to 90° C.; and / or,
[0029] The molecular weight of the thermoplastic acrylic resin is 50 kDa to 150 kDa; and / or;
[0030] The Tg of the thermoplastic acrylic resin is 80° C. to 110° C.; and / or,
[0031] The molecular weight of the polyester polyol resin is 800Da to 2000Da.
[0032] In some embodiments, the component A further contains one or more of a matting agent, a filler, a colorant, a dispersant, a leveling agent, and an anti-settling agent.
[0033] In some embodiments, in the component A,
[0034] The weight portion of the matting powder is 2 to 12 parts by weight; and / or,
[0035] The average particle size of the matting powder is 1 μm to 10 μm; and / or,
[0036] The filler has a weight portion of 2 to 10 weight portions; and / or,
[0037] The average particle size of the filler is 1 μm to 10 μm; and / or,
[0038] The weight proportion of the colorant is 2 to 9 parts by weight; and / or,
[0039] The colorant is high-pigment carbon black, and the average particle size of the high-pigment carbon black is 5nm to 30nm; and / or
[0040] The weight portion of the dispersant is 0.5 to 5 weight portions; and / or,
[0041] The weight proportion of the leveling agent is 0.5 to 5 weight proportions; and / or,
[0042] The leveling agent is selected from silicone and / or acrylate; and / or,
[0043] The anti-settling agent is present in an amount of 0.2 to 2 parts by weight.
[0044] In some embodiments, the polyisocyanate curing agent comprises polyisocyanate
[0045] The NCO functionality of the polyisocyanate is selected from 10 to 100; and / or,
[0046] The NCO content of the polyisocyanate is 25% to 30%; and / or,
[0047] The polyisocyanate has a structural unit shown in formula (I):
[0048] Wherein, R1 is H or methyl; R3 is C 1-8 Alkylene.
[0049] In some embodiments, the polyisocyanate curing agent comprises polyisocyanate,
[0050] The NCO functionality of the polyisocyanate is selected from 10 to 40; and / or,
[0051] The polyisocyanate also has a structural unit represented by formula (II):
[0052] Wherein, R2 is H or methyl; R4 is selected from one or more of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, hexyl, octyl, isooctyl, decyl, lauryl and isobornyl.
[0053] In some embodiments, in the component B, the polyisocyanate has a general structure as shown in formula (III):
[0054] wherein n is numerically equal to the NCO functionality of the polyisocyanate, n is selected from an integer ≥ 10, m is an integer selected from 0 to 5; R3 is -(CH2) a -; wherein a is 1, 2 or 3; "*" indicates the connection site.
[0055] In a second aspect of the present invention, a method for preparing a polyurethane coating is provided, using the polyurethane coating composition system described in the first aspect of the present invention, and the preparation method comprises the following steps:
[0056] Adding the thermoplastic acrylic resin to the first solvent in a medium-speed dispersion state, and dispersing at a high speed after the addition is completed, dispersing evenly until the particle fineness is ≤5 μm, to obtain a first resin solution;
[0057] Add the dispersant to the first resin solution, then add the colorant in a medium-speed dispersion state, add the filler, and then disperse at a high speed to disperse evenly until the particle fineness is ≤15 μm, to obtain a second resin solution;
[0058] Add the hydroxy acrylic resin and the polyester polyol resin to the second resin solution, disperse them uniformly, then add the matting powder in a medium-speed dispersion state, and after the addition is completed, perform high-speed dispersion to disperse uniformly until the particle fineness is ≤20 μm, to obtain a third resin solution;
[0059] Adding the leveling agent to the third resin solution, dispersing at a medium speed, and adjusting the viscosity to 40 Ku to 100 Ku using a second solvent to obtain the component A;
[0060] The component A, the component B and the component C are uniformly mixed according to corresponding weight ratios to prepare a polyurethane coating composition;
[0061] Spraying the polyurethane coating composition onto the surface of a plastic substrate to a film thickness of 15 μm to 25 μm, leaving it to level, and then drying it at 70° C. to 80° C. to form the polyurethane coating;
[0062] The dispersion speed of the medium-speed dispersion is 500rpm-600rpm, and the dispersion speed of the high-speed dispersion is 800rpm-1000rpm; the components of the first solvent and the second solvent are the same as the mixed solvent, and the total amount of the two constitutes the mixed solvent.
[0063] In the third aspect of the present invention, there is provided an application of the polyurethane coating combination system of the first aspect of the present invention on a plastic substrate, wherein the plastic substrate includes a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate and a PC / ABS composite plastic substrate.
[0064] In the fourth aspect of the present invention, a polyurethane coating product is provided, comprising a plastic substrate and a polyurethane coating layered on the surface of the plastic substrate, wherein the polyurethane coating is prepared by applying a polyurethane coating composition formulated from the polyurethane coating combination system described in the first aspect of the present invention onto the surface of the plastic substrate.
[0065] The inventors have found that the main reason why traditional PU coatings have poor chemical resistance (especially sunscreen resistance) is that the cross-linking density of PU coatings is low, resulting in insufficient density of the coating after curing, making it difficult to resist the erosion of chemical substances such as sunscreen (the main ingredient is small molecule substances such as octyl salicylate, which has a small molecular weight (250Da) and a high boiling point (331°C) and is difficult to volatilize, thus causing continuous erosion of the coating). Generally, the higher the SPF value of the sunscreen, the more difficult it is for the coating to tolerate; the main cause of bright marks is that the arrangement of the matting powder on the surface of the coating changes due to external scratches, affecting the originally uniform diffuse reflection effect. The denser the coating, the better the stability of the matting powder arrangement, that is, the better the scratch resistance, and vice versa. In the present application, by using a polyisocyanate having both high functionality (NCO functionality is preferably ≥10, and more preferably 10 to 100) and high isocyanate content (NCO content) as a curing agent, and cooperating with the hydroxyl-containing component (such as acrylic polyol resin), auxiliary agent, additive (such as colorant, filler, etc.) and other components in the main agent formula, the crosslinking ability of the coating system can be increased while reducing the amount of curing agent, so that the crosslinking network in the coating is tighter, thereby improving the density of the coating, and further improving the hardness, wear resistance and chemical resistance (sunscreen resistance) of the coating, and the adverse effect on the adhesion of the coating is small, while achieving the above-mentioned performance improvements, it can also maintain good adhesion. For the matte polyurethane coating combination system, it can effectively solve the shortcomings of the poor resistance to cream (such as sunscreen) and scratch resistance of the matte PU coating for automotive interiors, and can obtain a matte paint for automotive interiors with a delicate and uniform appearance, good chemical resistance and scratch resistance.
[0066] The polyisocyanate curing agent used in the present invention has a high NCO functionality, which can accelerate the cross-linking reaction between the hydroxyl-containing components of the coating system, shorten the baking time, reduce the film-forming time, and save energy. In addition, the polyisocyanate curing agent used also has the characteristics of high NCO content. Therefore, the molar ratio of -NCO:-OH to fully react (1 to 1.5):1 can be achieved by reducing the amount of curing agent added, so that the prepared polyurethane coating has improved hardness, wear resistance and chemical resistance.
[0067] The polyurethane coating combination system of the present invention and the polyurethane coating composition prepared therefrom can be used for surface coating of automobile interior parts, such as door panels, buttons, instrument panel sunshades and other interior parts. The polyurethane coating products prepared therefrom have improved hardness and wear resistance, good substrate adhesion, and can withstand SPF50+++ sunscreen cream and 100% octyl salicylate, while also meeting other various resistance test requirements. DETAILED DESCRIPTION
[0068] The present invention will be further described in detail below in conjunction with the embodiments and examples. It should be understood that these embodiments and examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive. It should also be understood that the present invention can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present invention, and the equivalent form obtained also falls within the protection scope of the present application. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present invention. It should be understood that the present invention can be implemented without one or more of these details.
[0069] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing implementation modes and embodiments and are not intended to limit the present invention.
[0070] the term
[0071] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0072] The terms "and / or", "or / and", and "and / or" used in this article include any one of two or more related listed items, and also include any and all combinations of related listed items, and the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in this application, the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution that is all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four of A, B, C, and D (that is, the technical solution that is all connected by "logical AND").
[0073] In the present invention, "plurality", "multiple", "multiple times", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0074] As used herein, "combination thereof", "any combination thereof", "any combination thereof" etc. include all suitable combinations of any two or more of the listed items.
[0075] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of the present invention, solve the technical problem of the present invention, and achieve the expected technical effect of the present invention.
[0076] Herein, "preferred", "better", "more preferred" and "suitable" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.
[0077] In the present invention, “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0078] In the present invention, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel solutions of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0079] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0080] In the present invention, the technical features described in an open format include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. It should be understood that when the chemical composition of a substance is described in a restrictive format, the substance may contain impurities present in a normal content, including but not limited to impurities inevitably introduced during the preparation process.
[0081] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0082] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0083] As used herein, the term "alkylene" refers to a hydrocarbon group having two monovalent radical centers derived from an alkyl group by removing two hydrogen atoms, which may be a saturated branched alkyl group or a saturated straight chain alkyl group. For example, "C1-C8 alkylene" or "C 1-8 "Alkylene" means that the alkyl portion contains 1 to 8 carbon atoms and each occurrence can be independently C1 alkylene, C2 alkylene, C3 alkylene, C4 alkylene, C5 alkylene, C6 alkylene, C7 alkylene or C8 alkylene. Suitable examples include, but are not limited to, methylene (-CH2-), 1,1-ethyl (-CH(CH3)-), 1,2-ethyl (-CH2CH2-), 1,1-propyl (-CH(CH2CH3)-), 1,2-propyl (-CH2CH(CH3)-), 1,3-propyl (-CH2CH2CH2-) and 1,4-butyl (-CH2CH2CH2CH2-).
[0084] As used herein, PU refers to polyurethane, hydroxyl is OH, VOC refers to volatile organic compound, Tg refers to glass transition temperature, NCO represents the group -N=C=O, PC substrate represents a substrate whose component is polycarbonate, and ABS substrate represents a terpolymer substrate composed of three monomers: acrylonitrile (A), butadiene (B), and styrene (S).
[0085] In the present invention, NCO content refers to the mass percentage of NCO groups in a certain mass of a sample.
[0086] The solid content in the present invention, unless otherwise specified, is expressed in mass percentage.
[0087] In the present invention, "molecular weight" generally refers to average molecular weight unless otherwise specified. It may be weight average molecular weight or number average molecular weight, but generally refers to weight average molecular weight unless otherwise specified.
[0088] In the present invention, "particle size" generally refers to the average particle size unless otherwise specified.
[0089] In the present invention, "room temperature" generally refers to 15°C to 35°C, and may further be 20°C to 30°C, unless otherwise specified.
[0090] In the present invention, the approximate numbers "about", "approximately", etc., unless otherwise specified, are allowed to fluctuate within a range of ±10%, and may further be ±5%, ±2%, etc. For example, about 20°C may be 20±2°C, 20±1°C, 20±0.5°C, etc. For example, a thickness of about 5 microns may be 5±0.5 microns, 5±0.2 microns, 5±0.1 microns, etc.
[0091] In the present invention, regarding "high pigment carbon black", in the art, according to the coloring ability of carbon black, it is generally divided into three categories, namely high pigment carbon black, medium pigment carbon black and low pigment carbon black.
[0092] The "boiling point" in the present invention refers to the initial boiling point unless otherwise specified.
[0093] In the present invention, "above" and "below" include the number itself unless otherwise specified.
[0094] A first aspect of the present invention
[0095] In the first aspect of the present invention, a polyurethane coating system (PU coating system) is provided, which uses a polyisocyanate with high functionality (NCO functionality is preferably ≥10, further preferably 10-100, and further can be 10-40) and high isocyanate content (NCO content ≥25%) as a curing agent, and cooperates with hydroxyl-containing components (such as acrylic polyol resins), auxiliary agents, additives (such as colorants, fillers, etc.) in the main agent formula to increase the cross-linking ability of the coating system, make the cross-linking network in the coating more compact, thereby improving the density of the coating, and can effectively solve the shortcomings of the polyurethane coating in terms of poor resistance to facial creams (such as sunscreen) and scratch resistance.
[0096] In some embodiments of the present invention, the composition comprises component A, component B and component C in a weight ratio of 100:(5-30):(70-100); component A provides a hydroxyl-containing component, component B is a polyisocyanate curing agent with high functionality (NCO functionality ≥10) and high NCO content (≥25%), and component C is used as a diluent. The three components cooperate with each other to form a polyurethane coating combination system with high crosslinking ability while reducing the amount of curing agent. The prepared polyurethane coating has improved hardness, wear resistance and chemical resistance (sunscreen resistance), can withstand SPF50+++ sunscreen cream, and can also withstand 100% octyl salicylate. In addition, it also has good substrate adhesion.
[0097] Component A
[0098] Component A includes hydroxy acrylic resin, thermoplastic acrylic resin, polyester polyol resin and solvent, wherein the solvent includes low boiling point solvent and high boiling point solvent, and component A may also contain one or more additives such as matting powder, filler, colorant, dispersant, leveling agent, anti-settling agent, etc.
[0099] In some embodiments, based on the total weight of component A being 100, component A comprises:
[0100]
[0101] In some preferred embodiments, based on the total weight of component A being 100, component A comprises:
[0102]
[0103] In some embodiments, based on the total weight of component A being 100, component A further comprises:
[0104]
[0105] The polyurethane coating combination system of the present invention can be a matte polyurethane coating combination system, and obtains a matte coating with a delicate and uniform appearance, good chemical resistance and scratch resistance.
[0106] In some preferred embodiments, based on the total weight of component A being 100, component A further comprises:
[0107]
[0108] Hydroxylated acrylic resin
[0109] Hydroxylated acrylic resin is the main film-forming resin in the polyurethane coating combination system and its coating products provided by the present invention, contains hydroxyl groups, has a large relative molecular weight, has good gloss and color retention, water and chemical resistance, dries quickly, is easy to construct, and is easy to recoat and rework.
[0110] The hydroxyl acrylic resin is the main hydroxyl-containing component in component A. In some embodiments, the hydroxyl value of the hydroxyl acrylic resin is 20 to 100 mgKOH / g, and can further be 30 to 80 mgKOH / g. The hydroxyl value of the hydroxyl acrylic resin is 20 mgKOH / g, 30 mgKOH / g, 40 mgKOH / g, 50 mgKOH / g, 60 mgKOH / g, 70 mgKOH / g, 80 mgKOH / g, 90 mgKOH / g, 100 mgKOH / g, etc.
[0111] Based on the total weight of component A being 100, the weight of the hydroxy acrylic resin in component A is preferably 20 to 50 parts by weight, and further can be 30 to 40 parts by weight, for example 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, and 50 parts by weight.
[0112] In some embodiments, the molecular weight of the hydroxy acrylic resin is 20 kDa to 100 kDa, and may further be 30 kDa to 80 kDa, for example, 20 kDa, 30 kDa, 40 kDa, 50 kDa, 60 kDa, 70 kDa, 80 kDa, 90 kDa, 100 kDa, etc.
[0113] In some embodiments, the glass transition temperature (Tg) of the hydroxy acrylic resin is 65°C to 100°C, and can further be 70°C to 90°C. The Tg of the hydroxy acrylic resin is, for example, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc. There is a certain correlation between the Tg of the hydroxy acrylic resin and the molecular weight. Selecting a hydroxy acrylic resin with both a suitable molecular weight and Tg is more conducive to construction, and is conducive to improving light retention and color retention, water resistance and chemical resistance, and film-forming efficiency.
[0114] In some embodiments, the hydroxylated acrylic resin may be selected from one or more of the following resin products: Hemmings FS-2451, Allnex 1184 SS-51、DIC WXU-880-BA, Mitsubishi Chemical CZ-1810, etc.
[0115] Thermoplastic acrylic resin
[0116] The thermoplastic resin used in component A is a non-reactive resin with a large relative molecular weight and excellent adhesion. It is used as an inert resin in the system to reduce curing shrinkage, improve adhesion, and is also beneficial for improving hardness. Since the Tg values of the thermoplastic acrylic resins are all higher than 90°C, they will not have an adverse effect on the hardness, scratch resistance and durability of the coating.
[0117] In some embodiments, the molecular weight of the thermoplastic resin in component A is 50 kDa to 200 kDa, and can further be 50 kDa to 150 kDa. Examples of molecular weights include 50 kDa, 60 kDa, 70 kDa, 80 kDa, 90 kDa, 100 kDa, 110 kDa, 120 kDa, 130 kDa, 140 kDa, 150 kDa, 160 kDa, 170 kDa, 180 kDa, 190 kDa, 200 kDa, and the like.
[0118] In some embodiments, the Tg of the thermoplastic resin in component A is 90° C. to 120° C., and may further be 90° C. to 110° C. The Tg of the thermoplastic resin is, for example, 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., and the like.
[0119] Based on the total weight of component A being 100, the weight of the thermoplastic resin in component A is preferably 2 to 10 parts by weight, and further can be 4 to 8 parts by weight. Examples of weight are 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. parts by weight.
[0120] In some embodiments, the thermoplastic resin in component A is selected from one or more of the following resin products: DSM B-805, DOW Paraloid A-11, DIC 56-1155, etc.
[0121] Polyester polyol resin
[0122] Polyester polyol resin is used as a flexible film-forming resin in component A. It has strong adhesion to plastic substrates such as PC and can significantly improve the flexibility and water resistance of the coating.
[0123] The polyester polyol resin is also one of the hydroxyl-containing components in component A. In some embodiments, the hydroxyl value of the polyester polyol resin in component A is 100 to 400 mgKOH / g, and can further be 100 to 350 mgKOH / g. The hydroxyl value of the polyester polyol resin in component A is, for example, 100 mgKOH / g, 150 mgKOH / g, 200 mgKOH / g, 250 mgKOH / g, 300 mgKOH / g, 350 mgKOH / g, 400 mgKOH / g, etc.
[0124] Based on the total weight of component A being 100, the weight of the polyester polyol resin in component A is preferably 2 to 10 parts by weight, and further can be 3 to 5 parts by weight. Examples of weight are 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. parts by weight.
[0125] The molecular weight of the polyester polyol resin in component A is relatively small. In some embodiments, the molecular weight of the polyester polyol resin in component A is 500Da to 5000Da, and can further be 800Da to 2000Da. The molecular weight of the polyester polyol resin in component A is 500Da, 1000Da, 1500Da, 2000Da, 3000Da, 4000Da, 5000Da, 6000Da, 7000Da, 8000Da, etc.
[0126] In some embodiments, the polyester polyol resin in component A is selected from one or more of the following resin products: Asahi Kasei Duranol T5651 (polycarbonate), Perstorp 4101 (polycaprolactone), WorléePol 1181 / 03, etc.
[0127] Synergy between resin components
[0128] Hydroxylated acrylic resin, thermoplastic acrylic resin, and polyester polyol resin are all resin components in component A. The three different resin components cooperate with each other in terms of molecular weight, hydroxyl value, Tg temperature, etc. to optimize the performance of the coating. Hydroxylated acrylic resin and polyester polyol resin are both hydroxyl-containing components, providing reactive hydroxyl groups (-OH) for cross-linking reaction with the curing agent.
[0129] The hydroxy acrylic resin provides the main film-forming resin, the polyester polyol resin provides the flexible film-forming resin, and the thermoplastic acrylic resin serves as a non-reactive resin. The three resin components have synergistic molecular weights, hydroxyl values, and glass transition temperatures, cooperate with each other, and work synergistically with the high-functionality polyisocyanate of the structure shown in formula (III), thereby comprehensively improving the resistance to sunscreen creams and the resistance to 100% octyl salicylate, while improving the hardness and abrasion resistance, and maintaining good substrate adhesion.
[0130] The relative molecular weight of hydroxyl acrylic resin is relatively large, and the hydroxyl value is relatively small, which is conducive to achieving better gloss and color retention, water and chemical resistance, fast drying, convenient construction, and easy recoating and rework; the relative molecular weight of polyester polyol resin is relatively small, and the hydroxyl value is relatively large. It has strong adhesion to plastic substrates such as PC and can significantly improve the flexibility and water resistance of the coating; the thermoplastic resin has a large relative molecular weight and excellent adhesion. It is used as an inert resin in the system to reduce curing shrinkage and improve adhesion. It is also beneficial to improve hardness, and has a high Tg value, which will not adversely affect the hardness, scratch resistance and durability of the coating.
[0131] If the molecular weight of the polyester polyol resin is too high, the coating system needs to add more solvent to dissolve it, which may easily lead to too low solid content of the system, unable to ensure film thickness, and not conducive to VOC control; if the molecular weight of the thermoplastic acrylic resin and hydroxy acrylic resin is too low, it may easily lead to poor density of the coating, resulting in gaps in the cured coating, which is easy to be corroded by chemicals.
[0132] If the hydroxyl value of the hydroxylated acrylic resin is too high, it may lead to poor adhesion of the coating to the substrate, or may lead to a low resin content in the formula, which in turn leads to too low solid content in the system, making it impossible to ensure film thickness, and at the same time prolonging the reaction time, affecting production efficiency. If the hydroxyl value of the polyester polyol resin is too low, it may have an adverse effect on the density of the coating.
[0133] The purpose of selecting the above Tg for the above different resin components is to ensure the hardness and drying speed of the coating. If the Tg is too high, the coating will be brittle; if the Tg is too low, the coating will be soft and dry too slowly, affecting production efficiency.
[0134] Solvents
[0135] The solvent in component A includes a low boiling point solvent and a high boiling point solvent.
[0136] The low boiling point solvent has a high volatilization rate, providing excellent solubility and quick drying. In some embodiments, the initial boiling point of the low boiling point solvent in component A is ≤100°C (i.e., below 100°C), more preferably 75°C to 100°C, for example 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.
[0137] In some embodiments, based on the total weight of component A as 100, the weight of the low boiling point solvent in component A is 10 to 40 parts by weight, and can further be 15 to 25 parts by weight, such as 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 28, 30, 35, 40 parts by weight. In some embodiments, the low boiling point solvent in component A is one or more of ethyl acetate (boiling point 77° C., relative volatility of 4), isopropyl acetate (boiling point 89° C.), butanone (boiling point 76.9° C.), etc.
[0138] The medium boiling point solvent can provide excellent solubility and lower substrate corrosion. In some embodiments, the initial boiling point of the medium boiling point solvent in component A is 100°C to 120°C, for example 100°C, 102°C, 105°C, 110°C, 112°C, 114°C, 115°C, 116°C, 117°C, 118°C, 120°C, etc.
[0139] In some embodiments, based on the total weight of component A as 100, the weight of the medium boiling point solvent in component A is 10 to 25 parts by weight, and can further be 10 to 20 parts by weight, for example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, etc. parts by weight. In some embodiments, the medium boiling point solvent in component A is one or more of n-butyl acetate (boiling point 117° C., relative volatility rate 1.5), isobutyl acetate (boiling point 116.5° C.), sec-butyl acetate (boiling point 112.3° C.), methyl isobutyl ketone (boiling point 117° C.), etc.
[0140] In some embodiments, the initial boiling point of the low boiling point solvent is ≤100°C, and the initial boiling point of the medium boiling point solvent is 100°C to 120°C.
[0141] Matting powder
[0142] The polyurethane coating system of the present invention may contain or may not contain matting powder.
[0143] The matting powder is a matting component. In the coating composition system of the present invention, it can cause diffuse reflection on the coating surface, thereby bringing about a matting effect, and a matte polyurethane coating composition can be prepared.
[0144] The matting powder used in the polyurethane coating system of the present invention may be organic or inorganic.
[0145] In the present invention, the particle size of the matting powder is controlled to be smaller in micrometer scale. In some embodiments, the average particle size of the matting powder is 1 μm to 10 μm, and further can be 2 μm to 5 μm, which is conducive to obtaining a more delicate and uniform matte effect. The average particle size of the matting powder is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.
[0146] In some embodiments, the matting powder is selected from Tosoh Tosou Evonik Grace HUBER One or more of the above.
[0147] The inventor found through a large number of experimental studies that Dongcao and Grace It is a SiO2 matting powder with special surface treatment, which can provide good hydrophobicity and chemical resistance. Spherical microparticles belonging to polymethyl urea resin are different from general inorganic matting powder. They contain -OH, which can participate in the cross-linking of the coating and have good scratch resistance, hardness and wear resistance.
[0148] In some embodiments, based on the total weight of component A being 100, the weight of the matting agent in component A is 2 to 12 parts by weight, and further can be 5 to 8 parts by weight. The weight of the matting agent in component A is, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. parts by weight.
[0149] filler
[0150] The polyurethane coating system of the present invention may contain fillers or may not contain fillers.
[0151] Fillers act as a skeleton in the coating prepared by the polyurethane coating combination system. By filling, the thickness of the coating is increased, the mechanical properties of the coating are improved, and the coating can have the effects of durability, corrosion resistance, heat insulation, and matting.
[0152] In some embodiments, the filler is selected from one or more of talc, barium sulfate, kaolin, mica powder, and the like.
[0153] The particle size of the filler is in a relatively small micrometer scale. In some embodiments, the average particle size of the filler is 1 μm to 10 μm, and further can be 2 μm to 5 μm, which is conducive to obtaining a more delicate and uniform appearance. The average particle size of the filler is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.
[0154] In some embodiments, based on the total weight of component A being 100, the weight of the filler in component A is 2 to 10 parts by weight, and further can be 3 to 8 parts by weight. The weight of the matting agent in component A is, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10 parts by weight.
[0155] Colorants
[0156] The polyurethane coating system of the present invention may or may not contain a colorant.
[0157] Adding colorant to the polyurethane coating system can play a coloring role.
[0158] In some embodiments, the average particle size of the colorant is 5 nm to 30 nm, and may further be 8 nm to 20 nm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 15 μm, 20 μm, 25 μm, etc.
[0159] In some embodiments, based on the total weight of component A being 100, the weight of the colorant in component A is 2 to 8 parts by weight, and further can be 3 to 5 parts by weight. The weight of the colorant in component A is, for example, 2, 3, 4, 5, 6, 7, 8, etc. parts by weight.
[0160] In some embodiments, the colorant is high-pigment carbon black, which has fine particles, high blackness, and better coloring effect. Further, the average particle size of the high-pigment carbon black is 5nm to 30nm, and further can be 8nm to 20nm. For example, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 15μm, 20μm, 25μm, etc.
[0161] In some embodiments, the colorant is a high-color carbon black selected from Orion COLOUR BLACK FW200, Orion SPECIAL BLACK 6, Cabot 1300, Cabot 1400, Bora Raven5000 Ultra III, etc.
[0162] Dispersants
[0163] The polyurethane coating system of the present invention may or may not contain a dispersant.
[0164] Adding dispersants to the polyurethane coating system can reduce the time and energy required to complete the dispersion process, reduce floating color, and improve tinting strength and storage stability.
[0165] In some embodiments, based on the total weight of component A being 100, the weight of the dispersant in component A is 0.5 to 5 parts by weight, and may further be 1 to 2 parts by weight. The weight of the colorant in component A is, for example, 0.5, 0.6, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, etc. parts by weight.
[0166] In some embodiments, the dispersant is selected from BASF One or more of BYK DISPERBYK-163, Lubrizol SOLSPERSE32500, etc.
[0167] Leveling agent
[0168] The polyurethane coating system of the present invention may contain or may not contain a leveling agent.
[0169] The addition of the leveling agent can make the coating flat, smooth and uniform, increase the orientation of the matting powder, reduce orange peel, and prevent the generation of Bénard cells. The leveling agent used in the present invention can be silicone or acrylate.
[0170] In some embodiments, based on the total weight of component A being 100, the weight of the leveling agent in component A is 0.5 to 5 parts by weight, and further can be 0.5 to 1 part by weight. The weight of the leveling agent in component A is, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, etc. parts by weight.
[0171] In some embodiments, the leveling agent is selected from BYK-306 (silicone), BYK-358N (acrylate), BASF (Acrylates), Evonik (silicone type) etc.
[0172] Anti-settling agent
[0173] The polyurethane coating system of the present invention may contain or may not contain an anti-settling agent.
[0174] By adding anti-settling agents, the thixotropy of the coating can be increased, forming a strong three-dimensional network structure in the system, which has anti-settling and anti-sagging effects.
[0175] In some embodiments, based on the total weight of component A being 100, the weight of the anti-settling agent in component A is 0.2 to 2 parts by weight, and further can be 0.5 to 1 part by weight. The weight of the anti-settling agent in component A is, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, etc. parts by weight.
[0176] In some embodiments, the anti-settling agent is selected from Hemmings DeuRheo229, 6900-20X, One or more of NS-5501, etc.
[0177] The types, particle sizes, and contents of various additives in component A cooperate with each other, and also cooperate with the cross-linked network formed by the resin component and the curing agent, to achieve better dense stacking, which is more conducive to improving the density and hardness of the coating, and can achieve better comprehensive performance of the coating, such as chemical resistance, resistance to creams (such as sunscreen), wear resistance, and scratch resistance.
[0178] Component B
[0179] The polyisocyanate curing agent in component B of the present invention comprises polyisocyanate, wherein the polyisocyanate contained is a polyisocyanate with high functionality (NCO functionality ≥ 10) and high NCO content (≥ 25%).
[0180] In some embodiments, component B is a polyisocyanate.
[0181] Component B is a polyisocyanate curing agent with high functionality (NCO functionality ≥ 10) and high NCO content (≥ 25%).
[0182] In the present invention, the "high functionality" of the polyisocyanate curing agent refers to a large number of NCO groups in the curing agent structure, which is numerically equal to the number of NCO groups contained in one molecule.
[0183] The NCO functionality of the polyisocyanate curing agent used in component B is ≥10, and can further be selected from 10 to 100, and can further be 10 to 40, and can also be 15 to 35; examples of NCO functionality are 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, etc. Unless otherwise specified, the NCO functionality in the present invention refers to the average value. In some embodiments, the NCO content of the polyisocyanate curing agent is ≥25%, and can further be 25% to 30%; examples of NCO content are 25%, 26%, 27%, 28%, 29%, 30%, etc.
[0184] In some embodiments, the NCO functionality of the polyisocyanate curing agent is ≥10 (preferably 6 to 100, and more preferably 10 to 40), and the NCO content is ≥25% (preferably 25% to 30%).
[0185] In some preferred embodiments, the NCO functionality of the polyisocyanate curing agent is ≥10, and the NCO content is 25% to 30%. At this time, the coating can also have improved compactness while reducing the amount of curing agent added. In order to avoid the coating being too hard and brittle, the NCO functionality of the polyisocyanate curing agent is preferably ≤100, and the NCO functionality is more preferably 10 to 40. That is, by controlling the NCO functionality of the polyisocyanate curing agent to 10 to 100, preferably 10 to 40, the resulting coating can better have both improved wear resistance, chemical resistance and good flexibility.
[0186] In some embodiments, the polyisocyanate has a structural unit represented by formula (I):
[0187] Wherein, R1 is H or methyl; R3 is C 1-8 Alkylene, for specific definition, please refer to the above term part. R3 can be a straight chain or branched structure, preferably a straight chain structure. In some embodiments, R1 is H. In some embodiments, R1 is methyl.
[0188] In some embodiments, the polyisocyanate further has a structural unit represented by formula (II):
[0189] Wherein, R2 is H or methyl; R4 is selected from one or more of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, hexyl, octyl, isooctyl, decyl, lauryl and isobornyl. In the molecule of the polyisocyanate curing agent, each occurrence of R4 may be the same or different.
[0190] In some embodiments, the polyisocyanate has a general structure as shown in formula (III):
[0191] wherein n is numerically equal to the NCO functionality of the polyisocyanate, n is selected from an integer ≥ 10, m is an integer selected from 0 to 5 (which may be 0, 1, 2, 3, 4 or 5); R3 is -(CH2) a-; wherein a is 1, 2 or 3; two "*" represent connection sites, which can be connected to other structural units or end groups in the molecule. In some embodiments, both "*" are connected to end groups. The structures such as formula (III) and their end groups in the present invention are clear to those skilled in the art. The end groups in formula (III) can be selected from the end groups that may be formed at the end of the polymerization reaction of acrylic monomers. In some embodiments, the end groups in formula (III) are selected from The terminal groups formed by polymerization, or and The end group formed during copolymerization. When m = 0, formula (III) is The definition of two “*” is consistent with the above, and further, both can be connected to terminal groups.
[0192] In some preferred embodiments, the polyisocyanate has a general structure as shown in formula (IV):
[0193] Wherein, n is numerically equal to the NCO functionality of the polyisocyanate, and n is selected from 10 to 40; the definitions of R3 and R1 are consistent with those above. Preferably, R3 is -(CH2) m -; wherein m is 1, 2, 3, 4, 5 or 6, further, m is 2, 4 or 6, further is 2.
[0194] In some embodiments of the present invention, the polyisocyanate in component B is a general structure shown in formula (V):
[0195] Wherein, any "*" is independently an end group formed by polymerization of acrylic monomers, and the two "*" may be the same or different; the definitions of n, R3, and R1 (including preferred embodiments and examples) are consistent with those described above.
[0196] The polyisocyanate curing agent used in component B can be prepared by the polymerization reaction of acrylic isocyanate. Acrylic isocyanate refers to a molecule having C=CC(=O)- at one end and an isocyanate group at the other end, for example The definition of R3 (including preferred and exemplary) is the same as above. Specific examples of acrylic isocyanate include ethyl isocyanate acrylate and ethyl isocyanate methacrylate. When the polymerization reaction is carried out, it is also possible to contain no or a small amount of Monomers can obtain polyisocyanates of the structure shown in formula (III).
[0197] By controlling the degree of polymerization and the size of the R3 and R1 groups (especially the size of the R3 group), the NCO functionality and NCO content of the polyisocyanate curing agent can be controlled. The greater the degree of polymerization, the higher the NCO functionality; if the R3 segment is too long or too heavy, the NCO content will decrease.
[0198] Component C (diluent)
[0199] Component C, as a diluent, can adjust the viscosity of the polyurethane coating system and regulate the film-forming process, such as film-forming time.
[0200] In some embodiments, component C is selected from one or more of ethyl acetate, acetone, isopropyl alcohol, diisobutyl ketone, and the like.
[0201] In some embodiments, component C is a mixture of ethyl acetate, acetone, isopropanol and diisobutyl ketone. Furthermore, the weight ratio of the above four components can be (5-10): (1-2): (2.5-5): (1.5-3).
[0202] In some embodiments, component C is a THD-51 type diluent.
[0203] Component A, Component B and Component C
[0204] In some embodiments, in the polyurethane coating system, the weight ratio of component A, component B and component C is 100:(5-30):(70-100), for example, 100:(5-25):(70-100), 100:(5-30):(70-90). The weight ratio of the three components can also be 100:8:80, 100:7:80, 100:6:80, 100:5.5:80, etc.
[0205] Based on 100 parts by weight of component A, the amount of component B can be 5 to 30 parts by weight, and further can be 5 to 25 parts by weight. The amount of component B relative to 100 parts by weight of component A is, for example, 5, 6, 7, 8, 9, 10, 12, 15, 20, 25, 30, etc. parts by weight.
[0206] Based on 100 parts by weight of component A, the amount of component C can be 70 to 100 parts by weight, and further can be 70 to 90 parts by weight. The amount of component C relative to 100 parts by weight of component A can be 70, 75, 80, 85, 90, 95, 100, etc. parts by weight.
[0207] Reasonable control of the weight ratio of component A and component B can control the molar ratio of -NCO to -OH in an appropriate ratio, which is more conducive to the full reaction between the hydroxyl-containing component and the curing agent, and is more conducive to improving the coating density, chemical resistance, sunscreen resistance and hardness while maintaining good coating adhesion. In some embodiments of the present invention, the molar ratio of -NCO to -OH is (1 to 1.5):1, further can be (1.1 to 1.5):1, and further can be (1.4 to 1.5):1. Examples of the molar ratio are (1.1:1), (1.2:1), (1.3:1), (1.4:1), (1.5:1), etc.
[0208] If the amount of diluent is too little, it will be impossible to adjust to the required viscosity. If the amount is too much, the solid content of the coating system will be low, which is not conducive to film formation.
[0209] Packaging and usage
[0210] In the polyurethane coating combination system, component A, component B, and component C can be packaged separately or in combination. Preferably, component A and component B are packaged separately. For components containing multiple components, such as component A, each component can be further packaged separately. For example, in combination packaging, component A, component B, and component D can be pre-mixed with component C and then packaged.
[0211] When using the polyurethane coating system, the components are mixed according to the corresponding weight parts, dispersed evenly, and a polyurethane coating composition with a suitable viscosity is prepared for coating. A known suitable coating method can be used, including but not limited to spraying. The film thickness can be about 15 to 25 μm, for example 15 μm, 20 μm, 25 μm, etc. Before coating, a sieving treatment can also be performed to remove insoluble particles.
[0212] It should be understood that since component A, component B, and component A can be weighed and mixed according to the required total weight and weight ratio when used, when each component is packaged independently, the weight ratio of the four components does not need to be strictly in accordance with the weight ratio in the aforementioned guidelines, as long as the packaging provided can provide a coating system for preparing the aforementioned weight ratio.
[0213] Second aspect of the present invention
[0214] In a second aspect of the present invention, a method for preparing a polyurethane coating is provided, wherein the polyurethane coating is prepared using the polyurethane coating combination system described in the first aspect of the present invention.
[0215] In some embodiments, the preparation method comprises the following steps:
[0216] In a medium-speed dispersion state, adding a thermoplastic acrylic resin to the first solvent (preferably slowly adding), and after the addition is completed, performing high-speed dispersion to disperse uniformly until the particle fineness is ≤5 μm, to obtain a first resin solution;
[0217] Add the dispersant to the first resin solution, then add the colorant (preferably slowly) and filler (preferably slowly) in a medium-speed dispersion state, and then disperse at a high speed to disperse evenly until the particle fineness is ≤15 μm, to obtain a second resin solution;
[0218] Add hydroxy acrylic resin and polyester polyol resin to the second resin solution, disperse them evenly, then add matting powder in a medium-speed dispersion state (preferably slowly), and after the addition is completed, disperse them evenly at high speed until the particle fineness is ≤20 μm, to obtain a third resin solution;
[0219] Add a leveling agent to the third resin solution, disperse at a medium speed, and use a second solvent to adjust the viscosity to 40 Ku to 100 Ku (Stormer viscometer test) to obtain component A;
[0220] The component A, the component B and the component C are uniformly mixed according to the corresponding weight ratio to prepare a polyurethane coating composition;
[0221] Spraying the polyurethane coating composition onto the surface of the plastic substrate to a film thickness of 15 μm to 25 μm, leaving it to level (it can be left to level at room temperature), and then drying it at 70° C. to 80° C. to form a polyurethane coating;
[0222] Among them, the dispersion speed of medium-speed dispersion is 500rpm~600rpm, and the dispersion speed of high-speed dispersion is 800rpm~1000rpm; the components of the first solvent and the second solvent are the same as the mixed solvent, and the total amount of the two constitutes the mixed solvent.
[0223] In some embodiments, the order of adding the colorant and the filler is not particularly limited. The colorant may be added first and then the filler, or the filler may be added first and then the colorant, or the colorant and the filler may be added at the same time.
[0224] In some embodiments, the viscosity of the prepared component A is, for example, 40Ku, 45Ku, 50Ku, 60Ku, 70Ku, 80Ku, 90Ku, 100Ku, etc.
[0225] In some embodiments, the polyurethane coating composition is sprayed using an Iwata W-101 spray gun, and further, the caliber is 1.0 mm.
[0226] In some embodiments, the film thickness of the spray coating is 15 microns, 20 microns, 25 microns, etc. The coating thickness after drying and film formation is substantially consistent with the thickness of the spray film. In some embodiments, the film thickness of the polyurethane coating after film formation is 15 microns, 20 microns, 25 microns, etc.
[0227] In some embodiments, the room temperature is 20°C to 30°C, and may be 20°C, 21°C, 22°C, 24°C, 25°C, 26°C, 28°C, 30°C, etc. The room temperature is also 23°C to 25°C.
[0228] In some embodiments, the spraying is followed by drying in an oven at a temperature of 70°C to 80°C, for example 70°C, 72°C, 74°C, 75°C, 76°C, 78°C, 80°C, etc.
[0229] The third aspect of the present invention
[0230] In the third aspect of the present invention, there is provided a use of the polyurethane coating combination system according to the first aspect of the present invention.
[0231] In some embodiments, the application includes but is not limited to application on a plastic substrate. Application on a plastic substrate; further, the plastic substrate includes but is not limited to a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate, and a PC / ABS composite material plastic substrate.
[0232] In some embodiments, the polyurethane coating system provided in the first aspect of the present invention includes but is not limited to application in automotive interior materials, and the polyurethane coating system is preferably a matte polyurethane coating system including a matting powder.
[0233] A fourth aspect of the present invention
[0234] In a fourth aspect of the present invention, a polyurethane coating product is provided, comprising a plastic substrate and a polyurethane coating layered on the surface of the plastic substrate, wherein the polyurethane coating is prepared by coating the polyurethane coating composition prepared by the polyurethane coating system of the first aspect of the present invention on the surface of the plastic substrate, and can be prepared by the preparation method of the second aspect of the present invention. Specific embodiments
[0236] The embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are preferably referred to the guidance provided in the present invention, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0237] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.
[0238] In the following examples, unless otherwise specified, the room temperature is 20°C to 30°C.
[0239] 1. Raw materials and reagents
[0240] 1.1. Preparation of polyisocyanates (high NCO functionality and high NCO content)
[0241] Some exemplary high-functionality polyisocyanates have the structure shown in formula (V) or formula (III):
[0242]
[0243] In formula (V), the two "*" are each independently The terminal groups generated during the polymerization reaction are as follows: R1 is H or methyl, R3 is ethylene, and n is 10, 15, 20, 25, 30, and 35. The structures of the polyisocyanates represented by formula (V) in the following examples are shown in Table 2.
[0244] by The high-functionality polyisocyanate is prepared by polymerization of a monomer (the monomer used here is ethyl isocyanate). The length of time for the polymerization reaction can be monitored by infrared detection of the residual amount of carbon-carbon double bonds. The carbon-carbon double bonds involved here are CH2=CH- or CH2-C(CH3)-. Detection 1640cm -1 Characteristic infrared peaks at the location.
[0245] Taking n as an example, the preparation process is as follows: 20g of ethyl acetate (the solvent needs to be dehydrated) is added to the reactor, stirring is started, and the temperature is slowly raised to 70°C. 20g of ethyl isocyanate is dissolved in ethyl acetate, 0.3g of initiator AIBN is added, and the mixture is slowly dripped into the reactor. After the dripping is completed, the infrared 1640cm -1 After confirming that all double bonds have reacted, the reaction is terminated to obtain a polyisocyanate product P0a.
[0246] The structure of product P0a was confirmed by hydrogen spectrum nuclear magnetic resonance: deuterated chloroform was used as solvent, and ppm was used as the chemical shift unit of characteristic peaks. 1In the H NMR spectrum, the positions of δ1.92-2.00 and 2.28-2.45 are hydrogen atoms on the main chain of the polymer, proving that a polymer has been formed; the positions of δ3.57-3.63 and 4.06-4.15 are continuous CH2 characteristic peaks.
[0247] In formula (III), the two "*" are each independently and The terminal groups formed during copolymerization, m is 1, 2, 3, 4, 5; R1 is H methyl, R2 is H or methyl, R3 is ethylene, R4 is methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, hexyl, n-octyl, isooctyl, decyl, lauryl or isobornyl. The structure of the polyisocyanate represented by formula (III) in the following examples is shown in Table 2.
[0248] by The high-functionality polyisocyanate is prepared by polymerization of monomers (the monomers used here are ethyl isocyanate and acrylate monomers). The length of time for the polymerization reaction can be monitored by infrared detection of the residual amount of carbon-carbon double bonds. The carbon-carbon double bond involved here is CH2=CH- or CH2-C(CH3). When the carbon-carbon double bond is CH2=CH-, the detection of 1640cm -1 Characteristic infrared peaks at the location.
[0249] The preparation process with n being about 12 and m being 1 is as follows: 20 g of ethyl acetate (the solvents all need to be dehydrated) is added to the reactor, stirring is started, and the temperature is slowly raised to 70°C. 18 g of ethyl isocyanate acrylate and 2 g of butyl methacrylate are dissolved in ethyl acetate, 1 g of initiator AIBN is added, and the mixture is slowly dripped into the reactor. After the dripping is completed, the infrared 1640 cm -1 After confirming that all double bonds have reacted, the reaction is terminated to obtain a polyisocyanate product P0b.
[0250] The structure of the product P0b was confirmed by hydrogen spectroscopy as follows: deuterated chloroform was used as solvent, ppm was used as the chemical shift unit of the characteristic peak, 1 In the H NMR spectrum: δ1.92-2.00, 2.28-2.45 are hydrogens on the polymer main chain, proving that a polymer has been formed; δ3.57-3.63, 4.06-4.15 are continuous CH2 characteristic peaks on the n unit structure; δ4.06-4.09 are CH2 characteristic peaks close to the O atom on the m unit structure; δ1.36-1.59 are continuous CH2 characteristic peaks on the m unit structure; δ0.95-0.99 are terminal CH3 characteristic peaks.
[0251] 1.2. Raw materials
[0252] 1.2.1. Raw materials of component A (main agent)
[0253] The types and amounts of the raw materials in component A used in the examples and comparative examples are shown in Table 1. The total weight of component A in each group is 100 g.
[0254] in, 1184 SS-51 is a hydroxy acrylic resin with a molecular weight of 50,000 Da, a hydroxyl value of 35 mg KOH / g, and a Tg of 90 °C;
[0255] FS-2451 is a hydroxy acrylic resin with a molecular weight of 50,000 Da, a hydroxyl value of 39.6 mg KOH / g, and a Tg of 93°C;
[0256] WorléePol 1181 / 03 is a polyester polyol resin with a molecular weight of 800Da and a hydroxyl value of 330mgKOH / g;
[0257] Duranol T5651 is a polyester (polycarbonate diol) resin with a molecular weight of 1000 Da and a hydroxyl value of 110 mg KOH / g;
[0258] Paraloid A-11 is a methacrylic resin with a molecular weight of 125,000 Da and a Tg of 100 °C;
[0259] B-805 is a methacrylic resin with a molecular weight of 85,000 Da and a Tg of 99°C;
[0260] Mitsubishi Chemical LR-7791 is a hydroxy acrylic resin with a molecular weight of 60,000 Da, a hydroxy value of 12 mg KOH / g (low hydroxy resin), and a Tg of 61°C.
[0261] Table 1. Types and amounts of raw materials in component A used in the examples and comparative examples.
[0262]
[0263]
[0264] The comparison results of Mitsubishi Chemical LR-7791 used as comparative example 3 show that even if a high-functionality curing agent is used, improper selection of the main resin of the component will lead to the failure to achieve the technical purpose of the present invention.
[0265] 1.2.2. Ratio of component A to component B
[0266] The relationship between the amounts of component A (main agent) and component B (curing agent) in each embodiment and comparative example is shown in Table 2.
[0267] The curing agent dosage is calculated as follows: NCO =(7.5×α×(V1×W1+V2×W2)) / (β×100). α is the molar ratio of -NCO to -OH in the system. V1 is the hydroxyl value of the hydroxy acrylic resin, and W1 is the resin percentage of the hydroxy acrylic resin. V2 is the hydroxyl value of the polyester polyol resin, and W2 is the resin percentage of the polyester polyol resin. β is the NCO content in the curing agent.
[0268] Table 2. Relationship between the dosage of component A (main agent) and component B (curing agent) in each embodiment and comparative example
[0269]
[0270] In Table 2, the unit of amount is g.
[0271] 2. Preparation of polyurethane coating
[0272] After mixing component A (Table 1) and component B according to the dosage ratio in Table 2, add THD-51 (diluent) of 80% by weight of component A, stir evenly and spray it onto the ABS+PC plastic substrate with an Iwata W-101 spray gun (caliber 1.0 mm). After the coating system is fully leveled, put it into an oven at 80°C to fully cure the system to obtain a coating to be tested with a thickness of 15μm to 25μm, and test the adhesion.
[0273] After the adhesion test of the coating to be tested, the coating is baked at 60°C for 48 hours and then tested for other items.
[0274] 3. Test items
[0275] The test results of each test item are shown in Table 3.
[0276] 3.1. Glossiness: Use a 60° angle gloss meter to test the coating glossiness, which is required to be within the range of 2±0.2.
[0277] 3.2. Adhesion test: ISO 2409-2013: 1mm grid and then test with tape, which is required to reach level 0.
[0278] 3.3. Hardness test: Mitsubishi UNI pencil, load 500g.
[0279] 3.4. Wear resistance test: Taber abrasion test, dry friction test and wet friction test were used to characterize the wear resistance of the coating.
[0280] 3.4.1. Taber abrasion test: CS-10 rubber, 500g load, the wear resistance of the coating is determined based on the number of friction circles, with no bottom exposure, and the upper limit is 1000 cycles.
[0281] 3.4.2. Dry friction: Determine the wear resistance of the coating based on the number of frictions, the wear level, and the gray card grade of the friction cloth. The more frictions, the smaller the wear level, and the larger the gray card grade of the friction cloth, which means the smaller the external friction marks and the better the friction resistance of the coating. The wear level is required to be ≤2, and the white cloth has no color change (according to the gray card grade of the friction cloth used for the test according to DIN EN 20105-A03 standard, the gray card fastness grade is required to be ≥4).
[0282] 3.4.3. Wet friction: Determine the wear resistance of the coating based on the number of frictions, wear level, and gray card grade of the friction cloth. The more frictions, the smaller the wear level, and the larger the gray card grade of the friction cloth, which means the smaller the external friction marks and the better the friction resistance of the coating. The wear level is required to be level 1, and the white cloth has no color change (according to the gray card grade of the friction cloth used for the test according to DIN EN 20105-A03 standard, the gray card fastness grade is required to be ≥ level 4).
[0283] 3.5. Boiling water test: To characterize the water resistance of the coating, the coating to be tested is placed in a 100°C water bath, taken out after 2 hours, and visually inspected for changes in appearance after cooling to room temperature. An adhesion test is also conducted, requiring no change in appearance and substrate adhesion ≤ Level 1.
[0284] 3.6. Chemical resistance: The drop test and cream resistance test were used to characterize the chemical resistance of the coating.
[0285] 3.6.1. Spot test: Synthetic sweat A (0.75% acetic acid by volume, prepared as follows: 7.5 mL of 100% acetic acid is added to distilled water to make up to 1 L), 0.1 mL of the solution is dropped on the surface of the coating to be tested with a pipette and exposed for 10 minutes. Dry in a high-temperature oven at 60°C for 30 minutes. Observe the coating surface after 24 hours. The coating appearance is required to have no visible changes.
[0286] 3.6.2. Face cream resistance test: Generally, the larger the SPF value of the face cream, the higher the test temperature and the longer the test time, the more difficult it is for the coating to withstand. Thierry GmbH sunscreen (popular type) and NIVEA SPF50+++ sunscreen were used respectively, and placed in a 100℃ high temperature box for 2h (test one) and 80℃ high temperature box for 24h (test two). The coating was required to have no changes in appearance and touch (such as lines, swelling, cracks, softening, and stickiness). Then the coating gray card grade was tested according to DIN EN 20105-A02 standard. A gray card grade of ≥4 indicates that there is no visual difference in color before and after the coating test, and there is no fading or flowery phenomenon. The substrate adhesion and scratch resistance were further tested.
[0287] 3.7. Scratch resistance: Newton pen (318 hardness tester), the scratch resistance of the coating is determined according to the spring force. The greater the bearing force and the absence of bottom exposure, the more scratch-resistant the coating is. The requirement is 9N and no bottom exposure.
[0288] 3.8. Hydrolysis test: To characterize the moisture and heat resistance of the coating, the coating to be tested is stored in a climate test chamber at 90±2℃ and 95±3% humidity for 72h. After the test, there should be no changes in appearance and touch (such as swelling, cracks, softening, and stickiness). Then, the color fastness grade is tested according to DIN EN 20105-A02 standard. The gray card grade is ≥4, indicating that there is no visible difference in color before and after the coating test, and there is no fading or flowery phenomenon. The coating substrate adhesion and scratch resistance are further tested.
[0289] 3.9. Dry heat resistance: Under the condition of 120℃*500h, the coating is required to have no changes in appearance and touch (such as lines, swelling, cracks, softening, stickiness), and then test its color fastness grade according to DIN EN 20105-A02 standard. The gray card grade is ≥4, which means that there is no visible difference in color before and after the coating test, and there is no fading or flowery phenomenon. Further test its adhesion and scratch resistance.
[0290] 3.10. Light test: According to the DIN 75220-D-IN1-T test standard, the coating to be tested is exposed to a light intensity of 830±80W / m 2 , placed in a sunlight simulation device at a temperature of 80±3℃ and humidity <30%RH for 240h. After the test, the coating is required to have no changes in appearance and touch (such as lines, swelling, cracks, softening, and stickiness), and then test its color fastness grade according to DIN EN 20105-A02 standard. The gray card grade is ≥4, indicating that there is no visible difference in color before and after the coating test, and there is no fading or flowery phenomenon. Further test its adhesion and scratch resistance.
[0291] 3.11. Storage stability: Before use, it is required to have no sinking to the bottom under the condition of 60℃×14 days (60℃×14d).
[0292] Table 3. Test results
[0293]
[0294]
[0295]
[0296] As can be seen from Table 1, Table 2 and Table 3, Example 1 and Comparative Example 1 keep other conditions unchanged, change the NCO content to 25% to 30%, and change the high-functionality polyisocyanate curing agent with a functionality of 6 or more. While reducing the amount of curing agent, the density of the coating can be greatly improved. The obtained polyurethane coating has improved hardness, wear resistance and chemical resistance, especially the tolerance of the coating to cream is greatly improved, and it can withstand the cream test with stricter conditions. At the same time, through the optimization of component A, the polyisocyanate curing agent with a functionality of preferably 10 to 100, more preferably 10 to 40, is used to make the obtained coating have good resistance and storage stability.
[0297] The technical features of the above-mentioned implementation modes and examples can be combined in any appropriate manner. To make the description concise, not all possible combinations of the technical features in the above-mentioned implementation modes and examples are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0298] The above-described embodiments only express several implementation methods of the present invention, which is convenient for understanding the technical solution of the present invention in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present invention, several variations and improvements can be made, which all belong to the protection scope of the present invention. In addition, it should be understood that after reading the above-mentioned teaching content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and the equivalent forms obtained also fall within the protection scope of this application. It should also be understood that the technical solutions obtained by those skilled in the art on the basis of the technical solution provided by the present invention through logical analysis, reasoning or limited experiments are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A polyurethane coating combination system, characterized in that: It comprises component A, component B and component C in a weight ratio of 100: (5-15): (75-90): The component A comprises a hydroxy acrylic resin, a thermoplastic acrylic resin, a polyester polyol resin and a mixed solvent; the mixed solvent comprises a low boiling point solvent having a boiling point below 100°C and a medium boiling point solvent having a boiling point of 100°C to 120°C; The component B is polyisocyanate, the NCO content of the polyisocyanate is 25%-30%, and the NCO functionality is 10-40; The component C is a diluent; In the component B, the polyisocyanate has a general structure shown in formula (III): (III); Wherein, n is numerically equal to the NCO functionality of the polyisocyanate, n is an integer selected from 10 to 40, and m is an integer selected from 0 to 2; "*" indicates a connection site; R1 is H or methyl; R2 is H or methyl; R3 is -(CH2) a -, wherein a is 2 or 3; R4 is selected from one or more of methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, lauryl and isobornyl; Taking the total weight of component A as 100 parts, the component A comprises: 20-50 parts by weight of hydroxy acrylic resin; 2-10 parts by weight of thermoplastic acrylic resin; 2-10 parts by weight of polyester polyol resin; 10 to 40 parts by weight of a low boiling point solvent; and 10-25 parts by weight of a medium boiling point solvent; in, The hydroxyl acrylic resin has a hydroxyl value of 30 to 80 mgKOH / g, a weight average molecular weight of 20 kDa to 100 kDa, and a Tg of 65°C to 100°C; The thermoplastic acrylic resin has a weight average molecular weight of 50 kDa to 200 kDa and a Tg of 90°C to 120°C; The polyester polyol resin has a hydroxyl value of 100 to 350 mgKOH / g and a weight average molecular weight of 500 Da to 5000 Da; The low boiling point solvent is one or more of ethyl acetate, isopropyl acetate and butanone; The medium boiling point solvent is one or more of n-butyl acetate, isobutyl acetate, sec-butyl acetate and methyl isobutyl ketone; In the polyurethane coating combination system, the molar ratio of -NCO to -OH is (1.1-1.5):
1.
2. The polyurethane coating combination system according to claim 1, characterized in that: In the component A, The weight average molecular weight of the hydroxy acrylic resin is 30 kDa to 80 kDa; and / or, The Tg of the hydroxy acrylic resin is 70°C to 90°C; and / or, The weight average molecular weight of the thermoplastic acrylic resin is 50 kDa to 150 kDa; and / or; The Tg of the thermoplastic acrylic resin is 90°C to 110°C; and / or, The weight average molecular weight of the polyester polyol resin is 800 Da to 2000 Da.
3. The polyurethane coating combination system according to claim 1, characterized in that: Based on 100 parts by weight of component A, the amount of component B is 5 to 10 parts by weight; Based on 100 parts by weight of component A, the amount of component C is 75 to 85 parts by weight.
4. The polyurethane coating combination system according to claim 1, characterized in that: The weight average molecular weight of the hydroxy acrylic resin is 40 kDa to 60 kDa; The hydroxy value of the hydroxy acrylic resin is 30 to 50 mgKOH / g; The Tg of the hydroxy acrylic resin is 85°C to 100°C; The weight average molecular weight of the thermoplastic acrylic resin is 80 kDa to 130 kDa; The Tg of the thermoplastic acrylic resin is 95°C to 110°C; The weight average molecular weight of the polyester polyol resin is 500 Da to 2000 Da; The hydroxyl value of the polyester polyol resin is 250 to 350 mgKOH / g; In the component A, based on 100 parts by weight of the total component A, the hydroxy acrylic resin is 30 to 40 parts by weight, the thermoplastic acrylic resin is 4 to 8 parts by weight, the polyester polyol resin is 3 to 5 parts by weight, the low boiling point solvent is 15 to 25 parts by weight, and the medium boiling point solvent is 10 to 20 parts by weight.
5. The polyurethane coating combination system according to claim 1, characterized in that: The component A further contains one or more of matting agent, filler, colorant, dispersant, leveling agent and anti-settling agent.
6. The polyurethane coating combination system according to claim 5, characterized in that: In the component A, The weight portion of the matting powder is 2 to 12 parts by weight; and / or, The average particle size of the matting powder is 1 μm to 10 μm; and / or, The filler has a weight portion of 2 to 10 parts by weight; and / or, The average particle size of the filler is 1 μm to 10 μm; and / or, The weight proportion of the colorant is 2 to 9 parts by weight; and / or, The colorant is high-pigment carbon black, and the average particle size of the high-pigment carbon black is 5 nm to 30 nm; and / or The dispersant has a weight portion of 0.5 to 5 weight portions; and / or, The weight proportion of the leveling agent is 0.5 to 5 weight proportions; and / or, The leveling agent is selected from silicone and / or acrylate; and / or, The anti-settling agent is present in an amount of 0.2 to 2 parts by weight.
7. The polyurethane coating system according to any one of claims 1 to 6, characterized in that: The NCO functionality of the polyisocyanate is 10-35.
8. The polyurethane coating system according to any one of claims 1 to 6, characterized in that: In the component B, R4 is selected from one or more of methyl, ethyl, propyl and butyl.
9. The polyurethane coating combination system according to claim 1, characterized in that: a is 2.
10. A method for preparing a polyurethane coating, characterized in that: A polyurethane coating system as claimed in any one of claims 1 to 9, wherein component A of the polyurethane coating system contains matting powder, filler, colorant, dispersant and leveling agent; The preparation method comprises the following steps: Adding the thermoplastic acrylic resin to the first solvent in a medium-speed dispersion state, and dispersing at a high speed after the addition is completed, dispersing evenly until the particle fineness is ≤5 μm, to obtain a first resin solution; Add the dispersant to the first resin solution, then add the colorant in a medium-speed dispersion state, add the filler, and then disperse at a high speed to disperse evenly until the particle fineness is ≤15 μm, to obtain a second resin solution; Add the hydroxy acrylic resin and the polyester polyol resin to the second resin solution, disperse them uniformly, then add the matting powder in a medium-speed dispersion state, and after the addition is completed, perform high-speed dispersion to disperse uniformly until the particle fineness is ≤20 μm, to obtain a third resin solution; Adding the leveling agent to the third resin solution, dispersing at a medium speed, and adjusting the viscosity to 40 Ku to 100 Ku using a second solvent to obtain the component A; The component A, the component B and the component C are uniformly mixed according to corresponding weight ratios to prepare a polyurethane coating composition; Spraying the polyurethane coating composition onto the surface of the substrate to a film thickness of 15 μm to 25 μm, leaving it to flow level, and then drying it at 70° C. to 80° C. to form the polyurethane coating; Among them, the dispersion speed of the medium-speed dispersion is 500 rpm ~ 600 rpm, and the dispersion speed of the high-speed dispersion is 800 rpm ~ 1000 rpm; the components of the first solvent and the second solvent are the same as the mixed solvent, and the total amount of the two constitutes the mixed solvent.
11. Use of the polyurethane coating combination system according to any one of claims 1 to 9 on a plastic substrate, wherein the plastic substrate comprises a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate and a PC / ABS composite material.
12. A polyurethane coated product, characterized in that: The invention comprises a plastic substrate and a polyurethane coating layered on the surface of the plastic substrate, wherein the polyurethane coating is prepared by coating a polyurethane coating composition prepared by the polyurethane coating combination system according to any one of claims 1 to 9 on the surface of the plastic substrate.