A binary / ternary nanoheterojunction and one-step preparation method and application thereof

The preparation process is simplified by one-step hydrothermal method, forming Cu2O/TiO2 and Cu/Cu2O/TiO2 nanoheterojunctions, solving the problems of complex equipment and low catalytic activity in the existing technology, achieving efficient photocatalytic performance, suitable for large-scale Large-scale production.

CN116422328BActive Publication Date: 2024-11-05SHANGHAI UNIVERSITY OF ELECTRIC POWER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310256118.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2024-11-05
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

In the prior art, when preparing binary Cu2O/TiO2 and ternary Cu/Cu2O/TiO2 nanoheterojunction composites, the equipment requirements are high and the process is complex, and it is not suitable for large-scale production, and the light response range is narrow and the catalytic activity is low.

Method used

By using one-step hydrothermal method, the divalent copper salt, organic reducing agent and titanium source are stirred and heated in an alkaline environment, the amount of fructose is controlled to reduce Cu2+ to Cu+, thereby forming Cu2O/TiO2 and Cu/Cu2O/TiO2 nanometers Heterojunction simplifies the process and improves catalytic performance.

Benefits of technology

Nanoheterojunction preparation with high yield and low equipment requirements has been achieved, photocatalytic performance has been improved, and good catalytic activity is shown in particular in visible light for water decomposition and CO2 reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116422328B_ABST
    Figure CN116422328B_ABST
Patent Text Reader

Abstract

The present invention relates to a binary / ternary nano heterojunction and a one-step preparation method and application thereof. The preparation method comprises the following steps: dissolving a divalent copper salt, an organic reducing agent and an alkali in water, stirring and dropping a titanium source; sealing the stirred solution, and heating for reaction; and centrifuging, washing and drying the reaction product to obtain a binary Cu2O / TiO2 and / or ternary Cu / Cu2O / TiO2 nano heterojunction. The nano heterojunction is used for photocatalytic decomposition of water to produce hydrogen and reduce CO2 under visible light. Compared with the prior art, the present invention reduces the production process, and the product prepared by the present invention has a morphological size of about 20nm and is evenly distributed, olive-shaped, and has good crystallinity. The binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nano heterojunction composite materials can greatly improve their photocatalytic performance by forming a heterostructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional nanomaterials, and in particular to a binary / ternary nano heterojunction and a one-step preparation method and application thereof. Background Art

[0002] Titanium dioxide is one of the most studied compounds in materials science. It is a semiconductor material with extremely low cost, strong chemical inertness and good photostability. Because of its good physical and chemical properties, it has become one of the most promising materials in terms of "energy" and "environment". It is widely used in photoelectrocatalytic hydrogen production, photocatalytic reduction of carbon dioxide, bacterial inactivation, dye degradation, etc., among which semiconductor photocatalytic technology is the most widely used. With solar energy as the excitation source, titanium dioxide generates photogenerated electron-hole pairs. Photogenerated electrons have high reducing properties, and hole pairs have strong oxidizing properties. Similarly, titanium dioxide as a photocatalytic material also has very significant disadvantages. The light response range of titanium dioxide materials is narrow, and the utilization rate of light is low; the band gap is too wide, and it is difficult to excite; photogenerated electron-hole pairs are easy to recombine, reducing catalytic activity, etc. These are current research difficulties.

[0003] In response to this problem, titanium dioxide and narrow bandgap cuprous oxide are used to form a pn heterostructure. Photogenerated electrons flow from the conduction band of cuprous oxide to the conduction band of titanium dioxide and gather, and holes gather in the valence band of cuprous oxide, which inhibits the rapid recombination of photogenerated electrons and holes, expands the light absorption range, and improves the photocatalytic activity. Patent CN115386941A first uses electrochemical anodic oxidation to obtain a titanium alloy sheet with titanium dioxide on the surface, and then prepares a titanium alloy sheet with titanium dioxide nanotubes on the surface by electrochemical cathode reduction, and finally uses a pulse deposition method to prepare a Cu2O / TiO2 composite material, which has high requirements for equipment and complex preparation procedures. Patent CN113181912A uses a two-step method to load cuprous oxide on hydrothermally formed titanium dioxide nanosheets. Compared with TiO2, its activity is increased by 1.64 times, and it can well degrade methyl orange (MO) wastewater solution under ultraviolet light, but its preparation method is time-consuming and requires hydrothermal reaction for 24 hours. Patent CN108355654A prepared a Cu / Cu2O / TiO2 composite visible light photocatalyst for the degradation of sulfamethoxazole solution, which has a good photocatalytic effect, but there are not many studies on photocatalytic water decomposition and CO2 reduction.

[0004] The above numerous preparation methods and ideas fully consider the improvement of photocatalytic performance of binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite materials, but most experimental methods have high equipment requirements and complex processes, which are not suitable for large-scale production. Therefore, it is still necessary to explore a simple, fast and high-yield method to prepare binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite materials. Summary of the invention

[0005] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and to provide a binary / ternary nanoheterojunction and a one-step preparation method and application thereof that can improve the production efficiency of binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite materials while reducing the production process.

[0006] The product prepared by the present invention has a size of about 20 nm and is evenly distributed, olive-shaped, and has good crystallinity. The binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nano-heterojunction composite materials can greatly improve their photocatalytic performance by forming a heterogeneous structure.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A one-step preparation method for a binary / ternary nano heterojunction, the method comprising the following steps:

[0009] Dissolve the divalent copper salt, organic reducing agent and alkali in water, stir and add the titanium source dropwise;

[0010] After the stirred solution is sealed, it is heated for reaction;

[0011] The reaction product is centrifuged, washed and dried to obtain a binary Cu2O / TiO2 and / or a ternary Cu / Cu2O / TiO2 nanoheterojunction.

[0012] In the one-step preparation process, Cu2O and TiO2 are generated simultaneously, which both promotes and restricts each other. By taking advantage of the reducing property of fructose in an alkaline environment, the amount of fructose is controlled to make Cu2O and TiO2 2+ Reduction to Cu + , and then by Cu + Reduction to Cu 0 , so the composition effect in the heterojunction can be controlled. Due to the change in the composition of the heterojunction, that is, the introduction of Cu into the Cu2O / TiO2 heterojunction affects the carrier transmission path in the original binary heterojunction and changes the band edge position in the heterojunction, so heterostructures with different compositions show different catalytic properties.

[0013] Furthermore, the divalent copper salt is copper acetate, the organic reducing agent is fructose, the alkali is sodium hydroxide, and the titanium source is tetrabutyl titanate.

[0014] Furthermore, the usage ratio of the divalent copper salt to the titanium source is (0.4-0.6) mmol:0.5 ml, preferably 0.5 mmol:0.5 ml.

[0015] Furthermore, the obtained product is a binary Cu2O / TiO2 nanoheterojunction, the molar ratio of the divalent copper salt to the organic reducing agent is between 5:1 and 10:3; the molar ratio of the divalent copper salt to the base is between 1:7 and 1:50.

[0016] Furthermore, the usage ratio of the divalent copper salt, the organic reducing agent, the base and the titanium source is 0.5 mmol: 0.15 mmol: 2.5 mmol: 0.5 ml.

[0017] Furthermore, the obtained product is a ternary Cu / Cu2O / TiO2 nanoheterojunction, the molar ratio of the divalent copper salt to the organic reducing agent is between 2:1 and 1:2; the molar ratio of the divalent copper salt to the base is between 0 and 1:5, and 0 is not taken.

[0018] Furthermore, the usage ratio of the divalent copper salt, the organic reducing agent, the base and the titanium source is 0.5mmol:1mmol:2.5mmol:0.5ml.

[0019] Furthermore, the heating reaction temperature is 160-200°C, and the time is 3-5h, preferably 180°C, 4h.

[0020] A binary / ternary nano heterojunction prepared by the method described above.

[0021] An application of the binary / ternary nanoheterojunction as described above, wherein the nanoheterojunction is applied to photocatalytic water decomposition to produce hydrogen and reduce CO2 under visible light.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] (1) The present invention adopts a one-step hydrothermal method for synthesis, which has low equipment requirements, is simple and efficient compared to the two-step process for preparation separately;

[0024] (2) In the composite nanomaterial prepared by the present invention, titanium dioxide, cuprous oxide and copper are in close contact, can form a heterogeneous structure, and have a large specific surface area. The two can better improve the performance of photoelectrocatalysis through synergistic effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1XRD characterization diagram of the binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nano-heterojunction composite material dispersions obtained in Example 1-2;

[0026] Figure 2 is a SEM characterization image of the binary Cu2O / TiO2 heterojunction composite material dispersion obtained in Example 1;

[0027] Figure 3 TEM characterization images of the binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite material dispersions obtained in Example 1-2;

[0028] Figure 4 is a HRTEM characterization image of the binary Cu2O / TiO2 heterojunction composite material dispersion obtained in Example 1;

[0029] Figure 5 The UV-visible absorption spectra and the converted bandgap width diagrams of the binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nano-heterojunction composite material dispersions obtained in Examples 1-2;

[0030] Figure 6 is a graph showing the amount of hydrogen produced by photocatalytic water decomposition of the binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite materials obtained in Example 1-2;

[0031] Figure 7 This is a graph showing the yield of CO, a product of photocatalytic reduction of carbon dioxide, by the binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunction composite materials obtained in Example 1-2. DETAILED DESCRIPTION

[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Unless otherwise specified in the present invention, % can be regarded as mass percentage.

[0033] A one-step method for preparing binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunctions comprises the following steps:

[0034] S1: Dissolve copper acetate, fructose and sodium hydroxide in deionized water, stir at room temperature and add tetrabutyl titanate dropwise; when preparing binary Cu2O / TiO2 nanoheterojunctions, the molar ratio of copper acetate to fructose is between 5:1 and 10:3, and the molar ratio of copper acetate to sodium hydroxide is between 1:7 and 1:50. When preparing ternary Cu / Cu2O / TiO2 nanoheterojunctions, the molar ratio of copper acetate to fructose is between 2:1 and 1:2. The molar ratio of copper acetate to sodium hydroxide is between 0 and 1:5. Tetrabutyl titanate is added dropwise under stirring, and the volume ratio of tetrabutyl titanate to deionized water during hydrolysis is between 1:100 and 1:50.

[0035] S2: After being stirred for a certain period of time, the solution is transferred to a stainless steel high-pressure reactor lined with polytetrafluoroethylene and sealed, and the reactor is placed in a forced air drying oven for heating;

[0036] S3: The product solution after cooling from room temperature is centrifuged and washed to pH 7, and dried to obtain binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunctions with a structure size between 10-20nm and good crystallinity. Binary Cu2O / TiO2 and ternary Cu / Cu2O / TiO2 nanoheterojunctions have good effects on photocatalytic water decomposition to produce hydrogen and reduce CO2 under visible light.

[0037] Example 1

[0038] A binary nano-heterojunction and a one-step preparation method and application thereof are as follows:

[0039] Weigh 0.5mmol copper acetate, 0.15mmol fructose and 2.5mmol sodium hydroxide, add them to 50ml deionized water in turn, stir magnetically at a speed of 1000rad / min, and add 0.5ml tetrabutyl titanate during stirring. Stir continuously for 30min at room temperature to promote the hydrolysis of tetrabutyl titanate. Transfer the stirred solution to a 100ml polytetrafluoroethylene-lined stainless steel autoclave and seal it. Place the autoclave in a blast drying oven and react at 180℃ for 4h. After cooling naturally to room temperature, centrifuge the reaction solution at 1500rad / min, wash it alternately with deionized water and anhydrous ethanol several times and centrifuge it. Place it in a blast drying oven and dry it thoroughly at 60℃ for 6h, and grind the product in a mortar. Obtain a binary Cu2O / TiO2 heterojunction composite material.

[0040] Take 5 mg of the product and add 4 ml of anhydrous ethanol, mix well and ultrasonicate for 10 min. Perform UV-visible absorption test.

[0041] Take 100 mg of the product and add it to 100 ml of 10% methanol solution, mix evenly and ultrasonicate for 10 minutes, put it into a photocatalytic reaction device, pass carrier gas for washing, evacuate and start xenon lamp irradiation; the generated gas is monitored online using a gas chromatograph, the detector is a TCD thermal conductivity detector, and the carrier gas is high-purity nitrogen.

[0042] Take 50 mg of the product and add it into 100 ml of deionized water. After magnetic stirring to mix evenly, put it into a photocatalytic reaction device. After evacuation, pass the carrier gas for washing, and start xenon lamp irradiation. The generated gas is monitored online using a gas chromatograph, the detector is a TCD thermal conductivity detector, and the carrier gas is high-purity nitrogen.

[0043] The XRD characterization results of the binary Cu2O / TiO2 heterojunction composite material prepared above are shown in Figure 1 The SEM, TEM and HRTEM analysis results of the binary Cu2O / TiO2 heterojunction composite material prepared above are shown in Figure 2 , Figure 3 (a) and Figure 4 .

[0044] The XRD diagram shows diffraction peaks of Cu2O at 36.4°, 42.3°, 61.4° and 73.5°, and the PDF card belongs to PDF#78-2076. There are diffraction peaks of TiO2 at 25.3°, 37.8°, 48.0°, 53.9°, 55.0°, 62.7°, 68.8°, 70.3° and 75.0°, and the PDF card belongs to PDF#21-1272.

[0045] SEM and TEM analysis showed that the binary Cu2O / TiO2 heterojunction composite material was uniformly distributed and the size was about 20nm. HRTEM analysis measured obvious Cu2O (111) crystal lattice and TiO2 (101) crystal lattice, which was consistent with XRD analysis.

[0046] Figure 5 The UV-visible absorption spectrum shows that it has good photoresponse under visible light and the bandgap is about 3.01 eV.

[0047] Compared with the ternary Cu / Cu2O / TiO2 nano-heterojunction composite material, it has better photocatalytic water decomposition hydrogen production ability and certain selective CO2 reduction ability, such as Figure 6-7 .

[0048] Example 2

[0049] A ternary nano-heterojunction and a one-step preparation method and application thereof are as follows:

[0050] Weigh 0.5mmol copper acetate, 1mmol fructose and 2.5mmol sodium hydroxide, add them to 50ml deionized water in turn, stir magnetically at a speed of 1000rad / min, and add 0.5ml tetrabutyl titanate during stirring. Stir continuously for 30min at room temperature to promote the hydrolysis of tetrabutyl titanate. Transfer the stirred solution to a 100ml polytetrafluoroethylene-lined stainless steel autoclave and seal it. Place the autoclave in a blast drying oven and react at 180℃ for 4h. After cooling naturally to room temperature, centrifuge the reaction solution at 1500rad / min, wash it alternately with deionized water and anhydrous ethanol several times and centrifuge it. Place it in a blast drying oven and dry it thoroughly at 60℃ for 6h, and grind the product in a mortar. A ternary Cu / Cu2O / TiO2 nano-heterojunction composite material is obtained.

[0051] Take 5 mg of the product and add 4 ml of anhydrous ethanol, mix well and ultrasonicate for 10 min. Perform UV-visible absorption test.

[0052] Take 100 mg of the product and add it to 100 ml of 10% methanol solution, mix evenly and ultrasonicate for 10 minutes, put it into a photocatalytic reaction device, pass carrier gas for washing, evacuate and start xenon lamp irradiation; the generated gas is monitored online using a gas chromatograph, the detector is a TCD thermal conductivity detector, and the carrier gas is high-purity nitrogen.

[0053] Take 50 mg of the product and add it into 100 ml of deionized water. After magnetic stirring to mix evenly, put it into a photocatalytic reaction device. After evacuation, pass the carrier gas for washing, and start xenon lamp irradiation. The generated gas is monitored online using a gas chromatograph, the detector is a TCD thermal conductivity detector, and the carrier gas is high-purity nitrogen.

[0054] The main difference between this embodiment and embodiment 1 is that the amount of fructose used in the reaction is changed, and single element Cu is introduced into the binary Cu2O / TiO2 heterojunction composite material, such as Figure 1 , forming a ternary Cu / Cu2O / TiO2 nanoheterojunction composite material.

[0055] There are diffraction peaks of Cu at 43.3°, 50.4°, 74.1° and 89.9°, and the PDF card is assigned to PDF#85-1326. TEM Figure 3 (b) The morphology shows that the particles are flaky and have a size of more than ten nanometers, which is significantly smaller than that in Example 1.

[0056] Due to the introduction of the surface plasmon resonance effect of Cu, its carrier transport mechanism is changed, and the light absorption capacity under visible light is better than that of Example 1, but the band gap is wider, such as Figure 5 .

[0057] Figure 6The photocatalytic performance of hydrogen production from water is lower than that of Example 1, but the selective reduction ability of CO2 under visible light has better catalytic activity than the binary Cu2O / TiO2 heterojunction composite material prepared in Example 1. Figure 7 This is because the introduction of Cu changes the original band edge position in the binary Cu2O / TiO2 heterojunction composite material, making it closer to the reduction band position of CO.

[0058] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. An application of a binary / ternary nanoheterojunction, characterized in that: The nanoheterojunction is used for photocatalytic water decomposition to produce hydrogen and reduce CO2 under visible light; The preparation method of the nano heterojunction comprises the following steps: Dissolve the divalent copper salt, organic reducing agent and alkali in water, stir and add the titanium source dropwise; After the stirred solution is sealed, it is heated for reaction; The reaction product is centrifuged, washed and dried to obtain a binary Cu2O / TiO2 and / or a ternary Cu / Cu2O / TiO2 nanoheterojunction; The obtained product is a binary Cu2O / TiO2 nanoheterojunction, the molar ratio of the divalent copper salt to the organic reducing agent is between 5:1 and 10:3; the molar ratio of the divalent copper salt to the base is between 1:7 and 1:50; The obtained product is a ternary Cu / Cu2O / TiO2 nanoheterojunction, the molar ratio of the divalent copper salt to the organic reducing agent is between 2:1 and 1:2; the molar ratio of the divalent copper salt to the base is between 0 and 1:5, and 0 is not taken.

2. The application of a binary / ternary nanoheterojunction according to claim 1, characterized in that: The divalent copper salt is copper acetate, the organic reducing agent is fructose, the alkali is sodium hydroxide, and the titanium source is tetrabutyl titanate.

3. The application of a binary / ternary nanoheterojunction according to claim 1, characterized in that: The usage ratio of the divalent copper salt to the titanium source is (0.4-0.6) mmol: 0.5 ml.

4. The application of a binary / ternary nanoheterojunction according to claim 1, characterized in that: The usage ratio of divalent copper salt, organic reducing agent, base and titanium source is 0.5 mmol: 0.15 mmol: 2.5 mmol: 0.5 ml.

5. The application of a binary / ternary nano heterojunction according to claim 1, characterized in that: The dosage ratio of divalent copper salt, organic reducing agent, base and titanium source is 0.5 mmol: 1 mmol: 2.5 mmol: 0.5 ml.

6. The use of a binary / ternary nanoheterojunction according to claim 1, characterized in that: The heating reaction temperature is 160-200° C. and the time is 3-5 h.