A non-energy radiant cooling coating and its preparation method and application
By modifying the combination of BaSO4 nanoparticles and acrylic resin and other components, the problem of poor compatibility between nanoparticles and polymers in radiation refrigeration coatings is solved, the reflectivity and mechanical properties of the coating are improved, and significant cooling efficiency improvement and coating are achieved. Layer hardness is enhanced.
Patent Information
- Application Number
- CN202310373162.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-10
AI Technical Summary
The existing radiation refrigeration coatings have limited their application due to poor compatibility and poor stability of nanoparticles and polymers, resulting in insufficient scattering intensity and low mechanical properties.
Modified BaSO4 nanoparticles were used to modify octadecyl trichlorosilane after reaction of titanium sulfate and H-β zeolite to form lipophilic titanium-containing zeolite, and coated on the surface of nano BaSO4, coupled with acrylic resin and silane. Components such as agents and emulsifiers are prepared to produce energy-consuming radiation-free refrigeration coatings.
The solar reflectivity and mechanical properties of the paint are significantly improved, the cooling efficiency is improved, the coating hardness and wear resistance are enhanced, and passive cooling can be achieved at a solar reflectivity of more than 96.5% and an atmospheric window emissivity of more than 95%.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of radiation cooling coatings, and in particular to a zero-energy radiation cooling coating, a preparation method thereof and an application thereof. Background Art
[0002] As the global climate continues to warm, the surface temperature rises, the urban heat island effect is greatly aggravated, and the temperature difference between urban and suburban areas increases significantly, which leads to an increase in the cooling load of buildings and a continuous increase in power consumption. Radiant cooling paint is a new type of paint that is applied to the surface of objects that need to dissipate heat and cool down. It can release the heat of the object in the form of thermal radiation, reduce the surface and internal temperature of the object, and thus achieve the purpose of cooling. The emergence of radiant cooling paint is expected to replace the air compression refrigeration system, which has positive significance for the world's energy structure and mitigation of global warming.
[0003] At present, the radiation cooling materials in the form of coatings are mainly paints with high refractive index nanoparticles wrapped in polymer resins and polymer scatterers with a fractional porous structure, which are generally selected from inorganic nanoparticles such as titanium dioxide, barium sulfate, and aluminum oxide. This type of material has two defects. First, the refractive index difference between the nanoparticles / pores and the polymer phase is small, resulting in insufficient scattering intensity and insufficient solar reflectivity; second, there is a large polarity difference between the nano-inorganic matter and the polymer matrix, so it is easy to agglomerate in the polymer and has poor dispersion, which reduces its mechanical properties and affects its application in production. This type of radiation cooling coating faces challenges in terms of stability and refractive index, which limits their application.
[0004] Therefore, developing energy-free radiative cooling coatings with long-term stability and high reflectivity is a difficult problem that needs to be overcome. Summary of the invention
[0005] Purpose of the invention: The purpose of the present invention is to provide an energy-free radiant cooling coating and its preparation method and application, so as to overcome the problems of poor compatibility and poor stability of polymer resin and inorganic nanoparticles in existing radiant cooling coatings, and to improve the mechanical properties and solar reflectivity of the coating.
[0006] The technical solution of the present invention:
[0007] A non-energy radiative cooling coating, comprising, by weight:
[0008] 20-35 parts of acrylic resin;
[0009] Silane coupling agent 1~5 parts;
[0010] Modified BaSO4 5~10 parts;
[0011] 1-8 parts of light calcium carbonate;
[0012] 1~2 parts of emulsifier;
[0013] Additives 0~12 parts;
[0014] 25-40 parts of solvent;
[0015] The modified BaSO4 is a nanoparticle having a titanium-containing zeolite shell and a nano BaSO4 core material.
[0016] In some embodiments, the acrylic resin is selected from one or more of pure acrylic resin, styrene acrylic resin, acetic acid acrylic resin, epoxy acrylic resin, polyurethane acrylic resin, silicone acrylic resin, fluorocarbon modified acrylic resin and silicone-acrylic hybrid acrylic resin.
[0017] In some embodiments, the silane coupling agent is selected from one or more of KH550, KH560, KH570, KH580, KH590, KH602, and KH792.
[0018] In some embodiments, the light calcium carbonate is common commercially available light calcium carbonate, which is specifically obtained by burning raw materials such as limestone to produce lime and carbon dioxide, adding water to digest the lime to produce lime milk, introducing carbon dioxide to carbonize the lime milk to produce calcium carbonate precipitate, and dehydrating, drying and crushing; the specifications of the light calcium carbonate are one or more of 600 mesh, 800 mesh, 1250 mesh, 1500 mesh, and 1800 mesh.
[0019] In some embodiments, the emulsifier is selected from one or more of sodium styrene sulfonate, polyoxypropylene glycerol ether, and nonylphenol polyoxyethylene ether.
[0020] In some embodiments, the auxiliary agent includes, but is not limited to, one or more selected from a dispersant, a defoaming agent, a film-forming aid, an antioxidant, a leveling agent, a defoaming agent, or a dye.
[0021] In some embodiments, the solvent is selected from at least one of ethyl acetate, butyl acetate, methyl isobutyl ketone, butanone, propylene glycol methyl ether acetate, isopropanol, and ethylene glycol monobutyl ether.
[0022] In some embodiments, the method for preparing the modified BaSO4 comprises:
[0023] 1) Dissolve titanium sulfate in water, stir magnetically to disperse evenly, add H-β zeolite, stir magnetically to react at room temperature for 24 h, and after the reaction is completed, transfer to a sand core funnel, filter, wash with distilled water until neutral, and dry to obtain titanium-containing β zeolite (hereinafter referred to as Ti-β);
[0024] 2) Take Ti-β, add it to a mixed solution of toluene and CCL4 containing octadecyltrichlorosilane, stir it magnetically at room temperature overnight, transfer it to a sand core funnel, filter it, wash it with CCl4 and ethanol respectively, and dry it to obtain an oleophilic titanium-containing β zeolite (hereinafter referred to as o-Ti-β);
[0025] 3) Nano-barium sulfate and the prepared o-Ti-β are placed in a three-necked flask, mixed and then sulfuric acid solution is added to adjust the pH. After the reaction is completed, the mixture is filtered, washed with deionized water and dried to obtain o-Ti-β@BaSO4 (hereinafter referred to as modified BaSO4).
[0026] In some embodiments, the particle size of the H-β zeolite is 200-400 mesh.
[0027] In some embodiments, the mass ratio of titanium sulfate to H-β zeolite is 1-5:10.
[0028] In some embodiments, the addition ratio of the Ti-β to octadecyltrichlorosilane is 1 g: 300-500 μmol.
[0029] In some embodiments, the mixed solution of toluene and CCL4 is a mixture of toluene and CCL4 in a mass ratio of 5-8:2-5.
[0030] In some embodiments, the mass ratio of the nano-BaSO4 and o-Ti-β is 1:1-4; the pH is adjusted by monitoring with an acidity meter and using sulfuric acid to regulate the pH value to maintain at 10-10.5.
[0031] On the other hand, the present invention also provides a method for preparing the energy-free radiation cooling coating as described above, comprising the following steps:
[0032] Preparation of emulsion raw materials: adding acrylic resin, emulsifier, and 50-70% by weight of solvent into an emulsification reactor and mixing them to form an emulsion raw material;
[0033] Preparation of radiation cooling coating: After the remaining solvent is mixed with modified BaSO4, silane coupling agent, light calcium carbonate and auxiliary agent, the above-mentioned emulsion raw materials are poured in and stirred to obtain the energy-free radiation cooling coating.
[0034] On the other hand, the present invention also provides an application of the energy-free radiant cooling coating as described above, comprising: coating the energy-free radiant cooling coating on a substrate, and forming a radiant cooling coating after the solvent evaporates; the coating is carried out by one or more of spraying, brushing or dipping methods.
[0035] Beneficial effects:
[0036] The present invention uses octadecyltrichlorosilane to modify Ti-β zeolite, and the hydrophilic groups on the surface of Ti-β zeolite are covered by hydrophobic silane groups, so that the obtained o-Ti-β is lipophilic; then the o-Ti-β is coated on the surface of nano BaSO4 to obtain hydrophobic and lipophilic modified nano BaSO4. The lipophilic modified nano BaSO4 is mixed with acrylic resin, silane coupling agent, emulsifier, etc. to prepare a radiation cooling coating, which can not only improve the solar reflectance of the coating, but also effectively increase the hardness of the coating and improve the wear resistance of the coating; at the same time, the present invention controls the coating degree of o-Ti-β on nano BaSO4 in the coating to adjust the balance between the stability and mechanical properties of the coating. The coating made of the energy-free radiation cooling coating of the present invention can increase the cooling temperature from about 3.1°C to about 10.5°C, and the cooling efficiency is significantly improved.
[0037] The preparation process of the energy-free radiation cooling coating of the present invention is convenient and simple to operate, and has low requirements on the working environment. The coating can be applied to the substrate by any of the spraying, brushing or dipping methods to form a radiation cooling coating. The radiation cooling layer has a sunlight reflectivity of about 96.5% or more, and can reach up to 98.5%; the atmospheric window emissivity is about 95% or more, and can reach up to 98.245%; so that the coating can passively cool down; at the same time, the coating surface has high hardness, good wear resistance and strong resistance to external environmental damage, and can resist the influence of external conditions such as sunlight, temperature changes, wind and rain on the coating, and has broad application prospects. DETAILED DESCRIPTION
[0038] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0039] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure. Titanium sulfate (96%, Shanghai Chemical Reagent Company) used in the examples is a chemically pure reagent; H-β zeolite (Si / AI=14) is provided by BASF, ground, and sieved through a 400-mesh sieve; octadecyltrichlorosilane (CAS: 112-04-9) is provided by Merck Sigma-Aldrich; light calcium carbonate specification 1500 mesh, purchased from Quanzhou Xufeng Powder Raw Material Co., Ltd.
[0040] Example 1
[0041] A non-energy radiant cooling coating comprises the following components in parts by mass: 20 parts of polyurethane acrylic resin, 3 parts of silane coupling agent KH580, 8 parts of modified BaSO4, 2 parts of emulsifier sodium styrene sulfonate, 30 parts of solvent ethyl acetate, 5 parts of dispersant Efka@FA 4654AN, 2 parts of film-forming aid Loxanol@CA 5308, and 5 parts of light calcium carbonate.
[0042] Add polyurethane acrylic resin, sodium styrene sulfonate, and 50-70% by weight of ethyl acetate into an emulsification reactor and mix them to form an emulsion raw material; mix the remaining ethyl acetate with modified BaSO4, and add light calcium carbonate, KH580, Efka@FA 4654AN and Loxanol@CA 5308 at the same time, stir, pour into the emulsion raw material and mix evenly, so as to obtain energy-free radiation refrigeration coating-1.
[0043] The preparation method of modified BaSO4 described in this embodiment is as follows:
[0044] 1) Weigh 0.3 g titanium sulfate and dissolve it in 10 mL water. Stir it magnetically for 10 min. Add 1 g H-β zeolite (325 mesh) and stir it magnetically for 24 h at room temperature. After the reaction is completed, transfer it to a sand core funnel, filter it, wash it with distilled water until it is neutral, and dry it at 100°C to obtain Ti-β.
[0045] 2) Weigh 1 g of the prepared Ti-β and add it to a mixed solution of toluene and CCL4 (toluene: CCL4 volume ratio = 8:2) containing 375 μmol of octadecyltrichlorosilane, and stir it magnetically at room temperature for 12 h. Transfer it to a sand core funnel, filter it, and then wash it with 50 mL CCl4 and 50 mL ethanol respectively. Dry it at 100°C to obtain o-Ti-β.
[0046] 3) Accurately weigh 2 g of nano-barium sulfate into a three-necked flask, add 3.2 g of prepared o-Ti-β, add sulfuric acid, control the pH value with a pH meter, and adjust the pH value to 10.2 with concentrated sulfuric acid. After the reaction is completed, filter, wash with deionized water and dry to obtain modified BaSO4.
[0047] Example 2
[0048] Example 2 refers to the implementation of Example 1, except that the weight percentages of the components of the energy-free radiation cooling coating are different. It includes: 30 parts of polyurethane acrylic resin, 1 part of silane coupling agent KH580, 10 parts of modified BaSO4, 2 parts of emulsifier sodium styrene sulfonate, 25 parts of solvent ethyl acetate, 5 parts of dispersant Efka@FA 4654AN, 3 parts of film-forming aid Loxanol@CA 5308, and 5 parts of light calcium carbonate.
[0049] The energy-free radiation cooling coating-2 was prepared.
[0050] Example 3
[0051] Example 3 refers to the implementation of Example 1, except that the weight percentages of the components of the energy-free radiation cooling coating are different, including: 35 parts of polyurethane acrylic resin, 5 parts of silane coupling agent KH580, 5 parts of modified BaSO4, 2 parts of emulsifier sodium styrene sulfonate, 25 parts of solvent ethyl acetate, 5 parts of dispersant Efka@FA 4654AN, 3 parts of film-forming aid Loxanol@CA 5308, and 5 parts of light calcium carbonate.
[0052] The energy-free radiation cooling coating-3 was prepared.
[0053] Example 4
[0054] Example 4 refers to the implementation method of Example 1, except that 200 mesh H-β zeolite is selected.
[0055] The energy-free radiation cooling coating-4 was prepared.
[0056] Example 5
[0057] Example 5 refers to the implementation method of Example 1, except that 400 mesh H-β zeolite is selected.
[0058] The energy-free radiation cooling coating-5 was prepared.
[0059] Example 6
[0060] Example 6 refers to the implementation method of Example 1, except that the amount of titanium sulfate added is 0.1 g.
[0061] The energy-free radiation cooling coating-6 was prepared.
[0062] Example 7
[0063] Example 7 refers to the implementation of Example 1, except that the amount of titanium sulfate added is 0.5 g.
[0064] The energy-free radiation cooling coating-7 was prepared.
[0065] Example 8
[0066] Example 8 refers to the implementation of Example 1, except that the added amount of octadecyltrichlorosilane is 300 μmol.
[0067] The energy-free radiation cooling coating-8 was prepared.
[0068] Example 9
[0069] Example 9 refers to the implementation of Example 1, except that the amount of octadecyltrichlorosilane added is 500 μmol.
[0070] The energy-free radiation cooling coating-9 was prepared.
[0071] Example 10
[0072] Example 10 refers to the implementation method of Example 1, except that the added amount of o-Ti-β is 2 g.
[0073] The energy-free radiation cooling coating-10 was prepared.
[0074] Embodiment 11
[0075] Example 11 refers to the implementation method of Example 1, except that the added amount of o-Ti-β is 5 g.
[0076] The energy-free radiation cooling coating-11 was prepared.
[0077] Comparative Example 1
[0078] Comparative Example 1 refers to the implementation of Example 1, except that the modified BaSO4 in the coating component is replaced with ordinary commercially available nano-BaSO4.
[0079] Coating-1 was prepared.
[0080] Comparative Example 2
[0081] Comparative Example 2 refers to the implementation of Example 1, except that the preparation method of the modified BaSO4 is as follows:
[0082] Accurately weigh 2 g of nano-barium sulfate into a three-necked flask, add 3.2 g of H-β zeolite (325 mesh), add sulfuric acid, control the pH value by an acidity meter, and adjust the pH value to 10.2 with concentrated sulfuric acid. After the reaction is completed, filter, wash with deionized water and dry to obtain H-β@BaSO4.
[0083] Coating-2 was prepared.
[0084] Comparative Example 3
[0085] Comparative Example 3 refers to the implementation of Example 1, except that the preparation method of the modified BaSO4 is as follows:
[0086] Weigh 0.3 g titanium sulfate and dissolve it in 10 mL water, stir it magnetically for 10 min. Add 1 g H-β zeolite (325 mesh), stir it magnetically at room temperature for 24 h, and after the reaction is completed, transfer it to a sand core funnel, filter it, wash it with distilled water until it is neutral, and dry it at 100°C to obtain Ti-β.
[0087] Accurately weigh 2 g of nano-barium sulfate into a three-necked flask, add 3.2 g of prepared Ti-β, add sulfuric acid, control the pH with a pH meter, and adjust the pH value to 10.2 with concentrated sulfuric acid. After the reaction is completed, filter, wash with deionized water and dry to obtain Ti-β@BaSO4.
[0088] Coating-3 was prepared.
[0089] Comparative Example 4
[0090] Coating-4 includes the following components in mass fractions: 45.5% of acrylic emulsion with a solid content of 48%, 22% of functional filler, 30% of deionized water, 1% of additive, and 1.5% of silane coupling agent solution with a mass fraction of 5%.
[0091] The functional filler is a mixture of a first filler and a second filler, wherein the first filler is a porous silica-zinc oxide-alumina composite particle with a particle size of 10 μm; the second filler is a mixture of barium sulfate and titanium dioxide powder in a mass ratio of 1:1, and the particle size of the second filler is 1 μm; the preparation method of the porous silica-zinc oxide-alumina composite particles is to dissolve sodium silicate, tetraethyl orthosilicate, zinc chloride and aluminum nitrate in a molar ratio of 1:1:0.5:0.5 in deionized water in turn to obtain a precursor solution; the precursor solution is transferred to a polytetrafluoroethylene reactor, the temperature is raised to 120°C and then the reaction is carried out at a constant temperature for 18 hours, and then the temperature is raised to 180°C and then the reaction is carried out at a constant temperature for 12 hours, and then cooled to room temperature to obtain a white precipitate, the white precipitate is washed with deionized water for 3 to 5 times, and then dried at 80°C to obtain the porous silica-zinc oxide-alumina composite particles; the mass ratio of the first filler to the second filler in the functional filler is 0.3:1.
[0092] The additives are composed of a film-forming aid, a dispersant, a leveling agent, a thickener, and a defoamer; the film-forming aid is an equal volume mixture of alcohol ester dodecaol and butyl carbitol, and the mass fraction of the film-forming aid in the water-based radiation refrigeration coating is 0.2%; the dispersant is an equal volume mixture of X-405 and Genapol ED3060, and the mass fraction of the dispersant in the water-based radiation refrigeration coating is 0.2%; the leveling agent is BYK341, and the mass fraction of the leveling agent in the water-based radiation refrigeration coating is 0.3%; the thickener is ASE6080, and the mass fraction of the thickener in the water-based radiation refrigeration coating is 0.2%; the defoamer is Silok4600, and the mass fraction of the defoamer in the water-based radiation refrigeration coating is 0.1%.
[0093] The preparation method of coating-4 described in this embodiment comprises the following steps:
[0094] (1) Polymer emulsion modification: acrylic emulsion, deionized water and silane coupling agent solution were weighed in proportion, and then the aqueous acrylic emulsion and part of the deionized water were stirred and mixed under magnetic stirring for 5 min, and then transferred to a high-speed disperser for high-speed stirring at a speed of 4000 r / min, and then 5% by mass silane coupling agent solution was slowly added at 50 °C for modification. The modification reaction time was 30 min, and then a polymer composite emulsion was obtained;
[0095] (2) Preparation of radiant cooling coating: Weigh the functional filler and additives in proportion, mix the functional filler and the remaining deionized water, and then heat to 50°C under magnetic stirring at a speed of 400 r / min and keep the temperature constant. Then slowly add the polymer composite emulsion obtained in step (1), continue stirring and mixing for 30 minutes, and then slowly add the film-forming additive, dispersant, leveling agent, thickener, defoaming agent and other additives in turn and continue stirring and mixing for 15 minutes to obtain coating-4.
[0096] The coatings prepared in the above examples and comparative examples were dip-coated on substrates respectively, and after the solvent evaporated, coatings 1 to 15 were formed respectively. The dry film thickness of the coatings was controlled to be 0.5 mm, and then the following properties of the coatings were tested. The results are shown in Table 1.
[0097] Solar reflectance: The reflectance of the coating was measured at an incident angle of 5° using a UV-visible-near infrared spectrophotometer Lambda950, with a wavelength range of 0.3~2.5 μm;
[0098] Atmospheric window emissivity: The atmospheric window emissivity of the coating is measured using an IR-2 dual-band emissivity tester with a wavelength range of 8~13 μm;
[0099] Coating adhesion: After baking the coating at 100°C for 24 hours, perform a cross-cut test in accordance with the national standard GB / T 9286-2021 Paints and varnishes.
[0100] Hardness: The hardness of the paint film is measured by the pencil method in accordance with the national standard GB / T 6793 2006 "Paints and varnishes";
[0101] Cooling effect: Apply black enamel and the above-mentioned coatings on aluminum sheets with a dry film thickness of about 0.5 mm. The room temperature is fixed at (25±1)℃. Use a 500 W infrared lamp to simulate sunlight to irradiate the coating. By adjusting the distance from the infrared lamp to the test plate, the temperature of the black enamel is controlled within the range of (37±1)℃. Use a surface thermometer to detect the back temperature of the test plate (T1) and the surface temperature of the coating (T2). Record the data every 10 minutes until the temperature stabilizes. Calculate the cooling temperature (△T) by the formula (△T=T2-T1).
[0102] Table 1 Performance test results of different coatings
[0103]
[0104] Zeolite itself is an inorganic substance with tiny holes and channels inside. Hydrophobic and lipophilic titanium-containing zeolite was synthesized by silanization modification. This lipophilic zeolite can greatly increase the solubility in organic matter. The crystal structure of the zeolite before and after modification has not changed. Silanization does not destroy the pore structure of the zeolite, but reduces the specific surface area and pore volume of the zeolite. Titanium enters the framework of the zeolite and becomes a four-coordinated framework, which increases the hydrophobic and lipophilic properties of the zeolite.
[0105] The above-prepared o-Ti-β zeolite is selected as a modifier to coat and modify nano BaSO4. The o-Ti-β zeolite forms a coating film on the surface of nano BaSO4. Under the experimental conditions of single-factor adjustment of titanium sulfate, octadecyl trichlorosilane and o-Ti-β, the coating effect under the optimal conditions is obtained. The coating layer is uniform, providing excellent dispersibility and lipophilicity for the modified nano BaSO4, and can be stably compatible in the radiation refrigeration coating for a long time. According to the test, the hydrophobic angle of the modified BaSO4 prepared by this method reaches 140°.
[0106] Add the modified BaSO4 filler, resin, silane coupling agent, emulsifier, solvent, light calcium carbonate and other additives into a mixer for mixing, and finally form a complete paint-like energy-free radiation cooling coating. The pore structure of H-β zeolite provides more radiation channels for the coating, and BaSO4 is used to further increase the refractive index and enhance the radiation cooling capacity of the coating; at the same time, the porous structure of H-β zeolite can not only improve the thermal insulation performance of the coating, but also increase the specific surface area of the modified BaSO4 filler, increase its bonding effect with the resin and other additives, and thus improve the mechanical properties of the coating.
[0107] The solar reflectivity of the radiant cooling coating is above 96.5%, and can reach up to 98.5%; the atmospheric window emissivity is above 95%, and can reach up to 98.245%; the cooling performance is excellent. The coating can be widely used in commercial and residential buildings, construction floor rooms, industrial plants, granaries / oil depots, cold chain logistics and other facilities that require refrigeration, with the advantages of low cost and large-scale production.
[0108] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a non-energy radiant cooling coating, It is characterized in that The following steps are involved: Preparation of emulsion raw materials: adding acrylic resin, emulsifier, and 50-70% by weight of solvent into an emulsification reactor and mixing them to form an emulsion raw material; Preparation of radiative cooling coatings: Residual solvent and modified BaSO 4 , silane coupling agent, light calcium carbonate and auxiliary agent are mixed, and then the above-mentioned emulsion raw materials are poured in and stirred evenly to obtain the energy-free radiation refrigeration coating; In terms of mass fraction, the energy-free radiation cooling coating comprises: Acrylic resin 20-35 parts; Silane coupling agent 1~5 parts; Modified BaSO 4 5~10 servings; 1-8 parts of light calcium carbonate; 1~2 parts of emulsifier; Additives 0~12 parts; 25-40 parts of solvent; The modified BaSO 4 It has a titanium-containing zeolite shell and nano-BaSO 4 Nanoparticles of core material; The modified BaSO 4 The preparation method comprises: 1) Mix and dissolve titanium sulfate and H-β zeolite, stir to react, filter after the reaction, wash and dry to obtain titanium-containing β zeolite; 2) adding the titanium-containing β-zeolite into a solution containing octadecyltrichlorosilane, stirring the solution for reaction, filtering and washing the solution to obtain the lipophilic titanium-containing β-zeolite; 3) Add nano BaSO 4 The prepared lipophilic titanium-containing β zeolite is added to a sulfuric acid solution for coating, and after coating, filtered, washed, and dried to obtain a modified BaSO 4 .
2. The method for preparing the energy-free radiation cooling coating according to claim 1, It is characterized in that The particle size of the H-β zeolite is 200-400 meshes.
3. The method for preparing the energy-free radiation cooling coating according to claim 1, It is characterized in that The mass ratio of the titanium sulfate to the H-β zeolite is 1-5:
10.
4. The method for preparing the energy-free radiation cooling coating according to claim 1, It is characterized in that The addition ratio of the titanium-containing beta zeolite to octadecyltrichlorosilane is 1 g: 300-500 μmol.
5. The method for preparing the energy-free radiation cooling coating according to claim 1, It is characterized in that The nano BaSO 4 The mass ratio of the oleophilic titanium-containing β-zeolite is 1:1~4.
6. A coating prepared by the method for preparing the energy-free radiation cooling coating according to any one of claims 1 to 5.
7. Application of a non-energy radiant cooling coating, It is characterized in that include: The coating according to claim 6 is applied on a substrate to form a coating after the solvent evaporates.
Citation Information
Patent Citations
High-temperature-resistant corrosion-resistant coating for aluminum plate
CN104017466A
Nano thixotropic agent and preparation method thereof
CN105623310A
Long-acting antibacterial radiation-proof negative oxygen ion far-infrared coating and preparation method thereof
CN112375445A
Synthesis method of Y zeolite-silicon oxide composite material with core-shell structure
CN114074945A
Water-based radiation refrigeration coating and preparation method thereof
CN114539861A
Cited By
Radiation refrigeration composition as well as preparation method and application thereof
CN121673874A