Polishing additive, polishing liquid, polishing method and battery preparation method

By adding oxidants, film-forming protectors, chelators and builders to the alkali distillation of PERC solar cells, a protective film is formed, which solves the problem of silicon oxide corrosion in the SE area, simplifies the process and reduces costs, and improves battery efficiency .

CN116445086BActive Publication Date: 2024-11-22SONGSHAN LAKE MATERIALS LAB +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210009444.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-11-22
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

The production process of existing PERC solar cells is complex and costly, especially in the alkali casting process, which easily leads to corrosion of silica in the SE area. Additional pre-oxidation processes are required to strengthen protection, which increases the process and cost.

Method used

Using a polishing additive containing an oxidant, a film-forming protector, a chelating agent and a builder, the process is simplified and cost-reducing by forming a dense protective film selectively adsorbed to the surface of the silicon oxide. .

Benefits of technology

The p-n junction in the SE region is effectively protected, the process flow is simplified, the production cost is reduced, and the battery efficiency is improved, so as to achieve alkali throwing operation without the pre-oxidation operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116445086B_ABST
    Figure CN116445086B_ABST
Patent Text Reader

Abstract

A polishing additive, a polishing liquid, a polishing method and a preparation method of a battery belong to the photovoltaic field. The polishing additive includes the following components by mass percentage: 0.2%-5% of an oxidant, 0.02%-1% of a film-forming protective agent, 0.1%-2% of a chelating agent, 0.1%-2% of a builder and the remainder of water. The polishing additive can be used to mix with an alkali solution to prepare a polishing liquid for making a SE-PERC solar cell, thereby simplifying the production process and reducing the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the photovoltaic field, and in particular, to a polishing additive, a polishing liquid, a polishing method and a method for preparing a battery. Background Art

[0002] Passivated Emitter and Rear Cell (PERC) has an extremely high cost-performance ratio and has therefore grown rapidly to become the mainstream high-efficiency crystalline silicon cell in the current photovoltaic market.

[0003] PERC requires polishing of the back of the cell to obtain a good passivation effect and increase the secondary reflection of the long-wavelength sunlight. The current mainstream SE-PERC manufacturing process based on Selective Emitter (SE) technology and PERC includes the following operations in sequence:

[0004] Texturing → diffusion → laser SE → front oxidation → single-sided dephosphorus silicon glass (PSG) → alkali polishing → post oxidation → coating → back laser grooving → screen printing → sintering test.

[0005] However, the above process has the problems of complicated procedures and high production cost. Summary of the invention

[0006] The present application provides a polishing additive, a polishing liquid, a polishing method and a method for preparing a battery. The polishing additive can protect silicon oxide, so when the polishing liquid prepared by the polishing additive is used to prepare a battery for alkaline polishing, the corrosion of silicon oxide can be reduced.

[0007] This application is implemented as follows:

[0008] In a first aspect, examples of the present application provide a polishing additive.

[0009] The polishing additive comprises the following components in percentage by mass:

[0010] 0.2%-5% oxidant, 0.02%-1% film-forming protective agent, 0.1%-2% chelating agent, 0.1%-2% builder and the balance water.

[0011] According to some examples of the present application, the polishing additive includes one or more of the following definitions:

[0012] First, the oxidant includes any one or more of sodium persulfate, ammonium persulfate and potassium persulfate;

[0013] The second limitation is that the film-forming protective agent includes glycerol and / or polyglycerol;

[0014] Thirdly, the chelating agent comprises sodium citrate;

[0015] Fourthly, the builder includes aminosulfonic acid.

[0016] In a second aspect, examples of the present application provide a polishing additive.

[0017] The polishing additive consists of the following components in mass fraction ratio: 0.5%-3% of sodium persulfate or ammonium persulfate, 0.05%-0.5% of glycerol, 0.5%-1% of sodium citrate, 0.5%-1% of aminosulfonic acid and the balance of deionized water.

[0018] In a third aspect, an example of the present application provides a polishing liquid comprising an alkaline solution and the above-mentioned polishing additive.

[0019] According to some examples of the present application, the alkali solution includes a sodium hydroxide solution or a potassium hydroxide solution; or, the alkali solution includes a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 1 wt % to 7 wt %.

[0020] According to some examples of the present application, the volume percentage of the polishing additive to the alkali solution is 0.5:100 to 2:100.

[0021] According to some examples of the present application, the use temperature of the polishing liquid is 60°C to 75°C.

[0022] In a fourth aspect, an example of the present application provides a polishing method for polishing the surface of crystalline silicon in a solar cell manufacturing process. The polishing method comprises: soaking crystalline silicon with surface silicon oxide in the above-mentioned polishing liquid at a temperature of 60° C. to 75° C. for 120 seconds to 240 seconds.

[0023] In the fifth aspect, the example of the present application provides a method for preparing a battery, wherein the battery is a SE-PERC solar cell, and the preparation method includes subjecting crystalline silicon to the following operations in sequence: texturing, diffusion, laser SE, single-sided dephosphorized silicon glass, alkali polishing, post-oxidation, coating, back laser grooving, screen printing and sintering, wherein the polishing liquid used in the alkali polishing operation is the aforementioned polishing liquid.

[0024] According to some examples of the present application, the preparation method further includes testing after sintering.

[0025] In the sixth aspect, the examples of the present application provide a use of glycerol or polyglycerol for preparing a polishing liquid, which is used for an alkali polishing operation, and the alkali polishing operation is implemented in the manufacturing process of solar cells; in the alkali polishing operation, the glycerol or polyglycerol forms a film by selectively adsorbing on the surface of silicon oxide, thereby protecting the silicon oxide.

[0026] In a seventh aspect, an example of the present application provides a polishing liquid comprising an alkali solution and a film-forming protective agent, wherein the film-forming protective agent comprises glycerol or polyglycerol.

[0027] In the above implementation process, the polishing additive provided in the embodiment of the present application has a film-forming protective agent that can selectively adsorb to the surface of silicon oxide and form a dense protective film, thereby preventing other reagents from eroding / corroding silicon oxide, thereby eliminating the need for additional protective operations. Since no additional protective operations are required, the use of the above polishing additives in the manufacture of solar cells is conducive to simplifying the process and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0029] Figure 1 This is a SEM image of the polished surface of the silicon wafer prepared in Example 1 of the present application;

[0030] Figure 2 This is a SEM image of the SE region on the front side of the silicon wafer prepared in Example 1 of the present application;

[0031] Figure 3 This is a SEM image of the polished surface of the silicon wafer prepared in Example 2 of the present application;

[0032] Figure 4 This is a SEM image of the SE region on the front side of the silicon wafer prepared in Example 2 of the present application;

[0033] Figure 5 This is a SEM image of the polished surface of the silicon wafer prepared in Example 3 of the present application;

[0034] Figure 6 This is a SEM image of the SE region on the front side of the silicon wafer prepared in Example 3 of the present application;

[0035] Figure 7 This is a SEM image of the polished surface of the silicon wafer prepared in Comparative Example 1 of the present application;

[0036] Figure 8 This is a SEM image of the SE region on the front side of the silicon wafer prepared in Comparative Example 1 of the present application;

[0037] Fig. 9 This is a SEM image of the polished surface of the silicon wafer prepared in Comparative Example 2 of the present application;

[0038] Fig.10 This is a SEM image of the SE area on the front side of the silicon wafer prepared in Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0039] As mentioned above, the manufacturing process of SE-PERC is texturing → diffusion → laser SE → front oxidation → single-sided dephosphorized silicon glass → alkali polishing → post oxidation → coating → back laser grooving → screen printing → sintering test.

[0040] The above process steps are complicated, resulting in great difficulty in implementation and high cost. After research, the inventors found that there is room for improvement in the above process. Specifically, the inventors believe that by improving the reagents in the above process, the process can be simplified, and thus the cost can be reduced.

[0041] In the examples, the inventors conducted an in-depth study on the alkaline polishing step in the above process and unexpectedly found that by improving the alkaline polishing liquid in the alkali polishing process, the "pre-oxidation" operation in the above process flow can be removed without adversely affecting the performance of the prepared battery. In some examples, the battery can even perform better.

[0042] The inventors' aforementioned improvements are based on the following understandings: in the above process, the alkali used in the alkali polishing process has a slow corrosion rate for silicon oxide, but a fast corrosion rate for silicon. Therefore, after single-sided PSG removal, the front side will not be corroded by the alkali solution due to the protection of silicon oxide, but the silicon exposed on the back side after the oxide layer is removed will be corroded by the alkali solution and polished.

[0043] In addition, due to the superposition of SE operation, the oxide layer in the area after laser SE is less protected and easily corroded by alkaline solution, resulting in battery failure. Therefore, a pre-oxidation process is added to the above process to strengthen the protection of silicon oxide in the SE area. In other words, according to the inventor of this application, pre-oxidation has become a key process step of SE-PERC cells.

[0044] In short, in the prior art, the SE operation on the front side of PERC will cause the SE region to be easily corroded by alkali solution, thereby destroying the pn junction in this region. Therefore, in order to be compatible with the SE process, an additional pre-oxidation process is required to strengthen the protection of the SE region, thereby increasing the preparation process and preparation cost.

[0045] In summary, in the existing SE-PERC cell manufacturing process, the pre-oxidation process has to be introduced due to the characteristics of the alkaline polishing solution used in the alkaline polishing process. Therefore, after recognizing the above facts, the inventors proposed a new polishing solution by improving the alkaline polishing solution used in the alkaline polishing process. The polishing solution can not only meet the needs of polishing, but also avoid the corrosion of silicon oxide in the SE region, so that the alkaline polishing operation can be completed without introducing a pre-oxidation operation.

[0046] Therefore, in the examples of the present application, a polishing additive, a polishing liquid, a polishing method and a method for preparing a battery are proposed.

[0047] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0048] At present, the alkaline polishing liquid commonly used in the manufacturing process of solar cells is, for example, an aqueous solution of sodium hydroxide or potassium hydroxide. The inventor of the present application has improved it and obtained a polishing liquid with an improved formula by proposing a polishing additive.

[0049] By using the polishing additive, the polishing liquid contains a chemical substance that can protect silicon oxide. In the example, the chemical substance is a component that can selectively adsorb silicon oxide to form a protective film on the surface of silicon oxide. Exemplarily, the chemical agent is glycerol (i.e., glycerol) or polyglycerol. Since the above-mentioned chemical substances are used in the polishing agent, they are adsorbed on the surface of silicon oxide to form a dense protective film, thereby blocking the corrosion of the alkaline polishing solution. Therefore, even in the absence of a pre-oxidation process, the SE area can be effectively protected.

[0050] Therefore, during the research, the inventors discovered that glycerol or polyglycerol can be used as a protective agent for silicon oxide by selectively adsorbing silicon oxide to form a film, and thus can be used in the polishing liquid used in the alkaline polishing operation of making solar cells.

[0051] Moreover, from the above analysis, it can be seen that, through the above scheme, the whole process is simplified because no pre-oxidation operation is required. Moreover, compared with the cost introduced by the pre-oxidation operation, the use of polishing additives is more economical - reducing the production cost. Moreover, since the pre-oxidation operation takes a relatively long time, the use of polishing additives can shorten the production cycle, thereby helping to increase production capacity.

[0052] In the example, the polishing additive of the alkali polishing liquid used in the alkali polishing operation includes the following components by mass percentage: 0.2%-5% of an oxidant, 0.02%-1% of a film-forming protective agent, 0.1-2% of a chelating agent, 0.1-2% of a builder, and the balance of water (which can be water of various appropriate purities, such as deionized water). The film-forming protective agent is the aforementioned chemical substance / component that can selectively adsorb silicon oxide to form a dense protective film on the surface of silicon oxide.

[0053] Wherein, the content of oxidant can be, for example, 0.5wt%, 1.1wt%, 1.3wt%, 1.8wt%, 2.4wt%, 2.8wt%, 3.6wt% or 4.7wt%. Wherein, the content of film-forming protective agent can be, for example, 0.03wt%, 0.05wt%, 0.08wt%, 0.1wt%, 0.3wt%, 0.4wt%, 0.6wt% or 0.8wt%. Wherein, the content of chelating agent can be, for example, 0.2wt%, 0.3wt%, 0.6wt%, 1.3wt%, 1.4wt%, 1.6wt%, 1.7wt% or 1.9wt%. Wherein, the content of builder can be, for example, 0.3wt%, 0.4wt%, 0.8wt%, 1.2wt%, 1.5wt%, 1.6wt%, 1.8wt% or 1.9wt%.

[0054] The polishing additives exemplified above not only use a film-forming protective agent, but also specifically add an oxidant, a chelating agent and a builder.

[0055] Among them, the oxidant can oxidize the impurities or pollutants that are difficult to remove, so that they are separated and enter the solution system and are therefore easy to remove. At the same time, the chelating agent can effectively chelate metal ions, reduce the metal impurity pollution of the silicon wafer, and improve the minority carrier life of the battery. The detergent has a cleaning effect on the silicon wafer and can effectively remove the dirt on the surface. Due to its strong wetting ability, it forms a coating on the removed impurities to prevent the impurities from causing secondary pollution to the silicon wafer surface.

[0056] Experiments have shown that the polishing additive can effectively protect the pn junction on the front side of the battery - for example, the SE area with a relatively thin oxide layer can also remain intact during the alkaline polishing process.

[0057] In the above-mentioned polishing additives, the oxidant includes but is not limited to any one or more of sodium persulfate, ammonium persulfate and potassium persulfate. For example, a mixture of two components - sodium persulfate and ammonium persulfate; or a mixture of three components - sodium persulfate, ammonium persulfate and potassium persulfate. The film-forming protective agent includes any one or a combination of two of glycerol (glycerol) and polyglycerol. The chelating agent includes sodium citrate, and the builder includes aminosulfonic acid.

[0058] Therefore, as an alternative polishing additive, the polishing additive is composed of the following components in mass fraction ratio: 0.5%-3% of sodium persulfate or ammonium persulfate, 0.05%-0.5% of glycerol, 0.5%-1% of sodium citrate, 0.5%-1% of aminosulfonic acid and the balance of deionized water.

[0059] Based on the above scheme, the example also proposes a polishing liquid including an alkali solution and a film-forming protective agent, wherein the film-forming protective agent includes glycerol or polyglycerol.

[0060] Further, other auxiliary examples may be introduced into the polishing liquid, such as one or more of the aforementioned chelating agent, builder and oxidant. Therefore, the polishing liquid in some examples includes alkali solution and the aforementioned polishing additive. The alkali solution is, for example, a strong alkali solution. For example, the alkali solution is a sodium hydroxide or potassium hydroxide solution.

[0061] In terms of concentration, the concentration of the sodium hydroxide solution or potassium hydroxide solution is, for example, 1 wt % to 7 wt %. Accordingly, the volume percentage of the polishing additive to the alkali solution is 0.5:100 to 2:100.

[0062] Based on the above polishing liquid, alkali polishing was verified and the results showed that it would be beneficial to use the polishing liquid at 60°C to 75°C (including but not limited to 61°C, 62°C, 64°C, 68°C, 70°C or 72°C).

[0063] Based on the polishing liquid, a polishing method can be implemented as follows, which is used to polish the surface of crystalline silicon in the solar cell preparation process. The polishing method includes: soaking crystalline silicon with surface silicon oxide in a polishing liquid at a temperature of 60° C. to 75° C. for 120 seconds to 240 seconds. Stirring and other operations can be used in combination during the soaking process.

[0064] Alternatively, a SE-PERC cell can be prepared based on the polishing liquid. SE-PERC refers to a solar cell based on a selective emitter, a passivated emitter and a back surface. In addition, the preparation method includes sequentially performing the following operations on crystalline silicon:

[0065] Texturing, diffusion, laser SE, single-sided dephosphorized silicon glass, alkali polishing, post-oxidation, coating, back laser grooving and screen printing, among which the alkali polishing operation uses the aforementioned polishing liquid. Furthermore, in order to ensure the performance of the battery or confirm whether it is qualified, a sintering test can also be performed after screen printing.

[0066] So far, the inventor has fully disclosed the solution of this application.

[0067] Single-sided polishing is a key process flow in the current mainstream SE-PERC battery, which has an absolute value improvement of 0.2% on the battery efficiency. By using the crystalline silicon polishing additive of this application, it is directly added to the alkaline polishing process tank during the polishing step, and the SE area on the front of the battery can be protected without the need for a pre-oxidation process. It is easy to know that the example solution of this application is aimed at the alkaline polishing link of the SE-PERC battery, and it achieves effective protection of the pn junction of the SE area without the need for a pre-oxidation process, and also simplifies the process flow, reduces costs and increases production capacity. On the other hand, because the polishing additive has an excellent cleaning effect, it can reduce impurity contamination on the surface of the silicon wafer, thereby improving the battery efficiency to a certain extent.

[0068] The present application is further described in detail below in conjunction with embodiments.

[0069] Example 1

[0070] 1. Prepare crystalline silicon polishing additives.

[0071] Calculated by mass percentage, 0.5% sodium persulfate, 0.05% glycerol, 0.5% sodium citrate, and 0.5% aminosulfonic acid are added to 98.45% deionized water, and the mixture is evenly mixed to prepare a polishing additive.

[0072] 2. Prepare a 5% sodium hydroxide alkaline solution.

[0073] 3. Take the crystalline silicon polishing additive prepared in step 1 and add it to the alkaline solution in step 2 at a volume ratio of 0.5% to obtain an alkaline polishing solution, and heat the alkaline polishing solution to 72°C.

[0074] 4. Immerse the silicon wafer that has undergone texturing, diffusion, laser SE and single-sided PSG removal in sequence (without pre-oxidation process) into the polishing solution prepared in step 3 and react for 240 seconds.

[0075] The scanning electron microscope image (SEM image) of the polished surface of the silicon wafer prepared in this embodiment is as follows: Figure 1 The scanning electron microscope image (SEM image) of the SE region on the front side of the silicon wafer prepared in this embodiment is shown in FIG. Figure 2 shown.

[0076] Example 2

[0077] 1. Prepare crystalline silicon polishing additives.

[0078] Calculated by mass percentage, 3% sodium persulfate, 0.5% glycerol, 1% sodium citrate and 1% aminosulfonic acid are added to 94.5% deionized water and mixed evenly to prepare an additive.

[0079] 2. Prepare a 5% sodium hydroxide alkaline solution.

[0080] 3. Take the crystalline silicon polishing additive prepared in step 1 and add it to the alkaline solution in step 2 at a volume ratio of 0.5% to obtain an alkaline polishing solution, and heat the alkaline polishing solution to 68°C.

[0081] 4. Immerse the silicon wafer that has undergone texturing, diffusion, laser SE and single-sided PSG removal in sequence (without pre-oxidation process) into the polishing solution prepared in step 3 and react for 200 seconds.

[0082] The scanning electron microscope image (SEM image) of the polished surface of the silicon wafer prepared in this embodiment is as follows: Figure 3 The scanning electron microscope image (SEM image) of the SE region on the front side of the silicon wafer prepared in this embodiment is shown in FIG. Figure 4 shown.

[0083] Example 3

[0084] 1. Prepare crystalline silicon polishing additives.

[0085] Calculated by mass percentage, 2% of ammonium persulfate, 0.2% of glycerol, 0.8% of sodium citrate, and 0.8% of aminosulfonic acid are added to 96.2% of deionized water, and the mixture is evenly mixed to prepare an additive.

[0086] 2. Prepare a sodium hydroxide alkaline solution with a mass percentage of 4.5%.

[0087] 3. Take the crystalline silicon polishing additive prepared in step 1 and add it to the alkaline solution in step 2 at a volume ratio of 0.5% to obtain an alkaline polishing solution, and heat the alkaline polishing solution to 68°C.

[0088] 4. Immerse the silicon wafer that has undergone texturing, diffusion, laser SE and single-sided PSG removal in sequence (without pre-oxidation process) into the polishing solution prepared in step 3 and react for 220 seconds.

[0089] The scanning electron microscope image (SEM image) of the polished surface of the silicon wafer prepared in this embodiment is as follows: Figure 5 The scanning electron microscope image (SEM image) of the SE region on the front side of the silicon wafer prepared in this embodiment is shown in FIG. Figure 6 shown.

[0090] Comparative Example 1

[0091] 1. Prepare a 5% sodium hydroxide alkaline solution and heat it to 68°C.

[0092] 2. Immerse the silicon wafer that has undergone texturing, diffusion, laser SE, front deoxidation and single-side PSG removal in the polishing liquid prepared in step 1 and react for 220 seconds.

[0093] The scanning electron microscope image (SEM image) of the polished surface of the silicon wafer prepared in this comparative example is as follows: Figure 7The scanning electron microscope image (SEM image) of the SE region on the front side of the silicon wafer prepared in this embodiment is shown in FIG. Figure 8 shown.

[0094] Comparative Example 2

[0095] 1. Prepare a 5% sodium hydroxide alkaline solution and heat it to 68°C.

[0096] 2. Immerse the silicon wafer that has undergone texturing, diffusion, laser SE and single-sided PSG removal (without pre-oxidation process) in the polishing solution prepared in step 1 and react for 220 seconds.

[0097] The operations of texturing, diffusion, laser SE and single-sided PSG removal in the above-mentioned embodiments and comparative examples are the same and adopt existing processes in the art, which will not be described in detail here.

[0098] The scanning electron microscope image (SEM image) of the polished surface of the silicon wafer prepared in this comparative example is as follows: Fig. 9 The scanning electron microscope image (SEM image) of the SE region on the front side of the silicon wafer prepared in this embodiment is shown in FIG. Fig.10 shown.

[0099] In the above drawings, Figure 1 , Figure 3 , Figure 5 , Figure 7 , Fig. 9 The polishing effect of the polished surface is shown, and the structure size is larger than that of the SE area on the front side. Figure 1 , Figure 3 , Figure 5 The polishing effect, that is, the flatness and uniformity of the polished surface are better than those of the control group. Figure 7 and Fig. 9 Better; Figure 2 , Figure 4 , Figure 6 , Figure 8 , Fig.10 The front SE area is shown, and the protection effect of the front SE is demonstrated through comparison. Figure 2 , Figure 4 , Figure 6 , Figure 8 and Fig.10 The comparison shows that Comparative Example 2 Fig.10 The top of the pyramid in the SE area is corroded and cannot provide effective protection.

[0100] Test Example 1

[0101] Performance Testing

[0102] The alkaline polished silicon wafers in Examples 1-3 and Comparative Examples 1-2 were sequentially subjected to post-oxidation, coating, back-side laser grooving, screen printing, and sintering to prepare SE-PERC solar cells and the solar cell performance was compared and tested. The specific results are shown in Table 1.

[0103] Table 1 Solar cell performance

[0104] <![CDATA[U oc (V)]]> <![CDATA[J sc (mA / cm 2 )]]> FF(%) <![CDATA[E ff (%)]]> Example 1 0.6882 40.89 81.81 23.022 Example 2 0.6891 40.92 81.68 23.032 Example 3 0.6895 40.95 81.72 23.074 Comparative Example 1 0.6885 40.90 81.73 23.015 Comparative Example 2 0.6831 40.87 81.50 22.753

[0105] According to Table 1 above, the efficiency of the PERC cell obtained by using the crystalline silicon polishing additive and polishing method of the present application is higher than the efficiency of the cell prepared by the conventional process (Comparative Example 1), and is also significantly better than the efficiency of the cell prepared by the process of Comparative Example 2 without pre-oxidation.

[0106] As shown in the accompanying drawings, the SE region of the silicon wafer after alkali polishing is still effectively protected by the additive of the present application without the pre-oxidation process. In addition, the polishing effect obtained by the additive of the present application, that is, the flatness and uniformity of the polished surface, is better than that of the comparative example.

[0107] Comparative Example 2 adopts conventional process without pre-oxidation process, and the SE region is severely corroded after alkali polishing, resulting in the destruction of the pn junction in this region. Therefore, the battery efficiency of Comparative Example 2 is much lower than that of other embodiments.

[0108] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A polishing additive, characterized in that: The polishing additive is composed of the following components by mass percentage: 0.2%-5% of an oxidant, 0.02%-1% of a film-forming protective agent, 0.1%-2% of a chelating agent, 0.1%-2% of a builder and the balance of water; The film-forming protective agent is glycerol and / or polyglycerol; The oxidant is any one or more of sodium persulfate, ammonium persulfate and potassium persulfate; The chelating agent is sodium citrate; The builder is aminosulfonic acid.

2. A polishing additive, characterized in that: The polishing additive consists of the following components in mass fraction ratio: 0.5%-3% of sodium persulfate or ammonium persulfate, 0.05%-0.5% of glycerol, 0.5%-1% of sodium citrate, 0.5%-1% of aminosulfonic acid and the balance of deionized water.

3. A polishing liquid, characterized in that: The polishing liquid consists of an alkali solution and the polishing additive according to claim 1 or 2.

4. The polishing liquid according to claim 3, characterized in that The alkali solution includes sodium hydroxide or potassium hydroxide solution.

5. The polishing liquid according to claim 4, characterized in that: The alkali solution includes a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 1wt% to 7wt%.

6. The polishing liquid according to claim 4, characterized in that The volume percentage of the polishing additive to the alkali solution is 0.5:100 to 2:

100.

7. The polishing liquid according to claim 4, characterized in that The use temperature of the polishing liquid is 60°C to 75°C.

8. A polishing method for polishing the surface of crystalline silicon in a solar cell manufacturing process, characterized in that: The polishing method comprises: immersing crystalline silicon with surface silicon oxide in the polishing liquid according to any one of claims 3 to 7 at a temperature of 60° C. to 75° C. for 120 seconds to 240 seconds.

9. A method for preparing a battery, wherein the battery is a SE-PERC solar cell, characterized in that: The preparation method comprises sequentially performing the following operations on crystalline silicon: Texturing, diffusion, laser SE, single-sided dephosphorized silicon glass, alkali polishing, post-oxidation, coating, back laser grooving, screen printing and sintering, wherein the polishing liquid used in the alkali polishing operation is the polishing liquid according to any one of claims 3 to 7.

10. The preparation method according to claim 9, characterized in that: The preparation method also includes testing performed after the sintering.

Citation Information

Patent Citations

  • Chemically mechanical polishing solution

    CN102533125A

  • Crystal silicon polishing additive and use method thereof for crystal silicon polishing

    CN107904663A

  • PERC battery back polishing additive and process

    CN110922970A

  • Polishing solution additive for back face of silicon slice, polishing solution, and polishing method of silicon slice of PERC crystalline silicon solar cell

    CN111015369A

  • PERC monocrystalline silicon solar cell and preparation method thereof

    CN111769175A