A method for preparing rare earth antibacterial stainless steel using copper smelting slag and rare earth antibacterial stainless steel
Through the deep reduction and deep desulfurization process, the problems of oxidative desulfurization and low copper utilization in preparing antibacterial stainless steel from copper smelting slag are solved, and the preparation of rare earth antibacterial stainless steel with high copper content and low cost is achieved, with stable performance and in line with industry standards.
Patent Information
- Application Number
- CN202310211185.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-07
AI Technical Summary
When using copper smelting slag to prepare antibacterial stainless steel, the existing technology has problems such as the need for oxidative desulfurization of the copper slag, low copper content in the tailing slag, low copper content in the copper-iron alloy, and low utilization rate.
Use deep reduction and deep desulfurization processes to form a copper-iron alloy, omit the oxidative desulfurization step, reduce the sulfur content through pre-desulfurizers and deep desulfurizers, increase the copper content of the copper-iron alloy, reduce the use of additives, and conduct it at low alkalinity and low reduction temperature Smelting and heat treatment to prepare rare earth antibacterial stainless steel.
It effectively increases the copper content of the copper-iron alloy, reduces the cost, avoids an increase in liquid phase temperature, improves the utilization rate of copper smelting slag, and prepares rare earth antibacterial stainless steel with stable performance and in line with industry standards.
Abstract
Description
Technical Field
[0001] The invention relates to the field of stainless steel preparation, in particular to a method for preparing rare earth antibacterial stainless steel by utilizing copper smelting slag and the rare earth antibacterial stainless steel. Background Art
[0002] Antibacterial stainless steel has the characteristics of smooth and stainless steel and good antibacterial property by adding antibacterial metal elements into the stainless steel matrix as a whole, so that it has both the smooth and stainless characteristics of ordinary stainless steel and good antibacterial property, and is widely used in the fields of medicine, daily use, food, marine engineering, etc. Antibacterial stainless steel is mainly divided into copper-containing antibacterial stainless steel and silver-containing antibacterial stainless steel. Since the former has a relatively low cost compared with the latter, it has been more widely used. CN105088092B discloses a new type of medical antibacterial stainless steel, and proposes to add an appropriate amount of Cu element and trace rare earth elements to stainless steel to obtain medical antibacterial stainless steel with good pitting resistance that has good antibacterial infection function and meets the requirements of surgical implantation. However, this method starts from the traditional stainless steel smelting raw materials, and the costs of Ni, Cr, Mn, etc. are relatively high. The addition of Cu and Re further increases the cost, and the metal is lost when added, and the composition is prone to unevenness.
[0003] At present, the production process mainly reduces production costs by smelting cheap iron / chromium / nickel / copper raw materials to obtain antibacterial stainless steel. Among them, copper smelting slag has become an important raw material for the preparation of antibacterial stainless steel because of its wide source.
[0004] Copper smelting slag is produced during the copper smelting process, and its main components are FeO and SiO2, and it contains a certain amount of copper and sulfur. In the traditional preparation process, copper smelting slag needs to be depleted at high temperature or flotation depleted to recover copper matte before it can be discarded or piled up, and the iron and residual copper (0.3-1%) in the tailings cannot be fully utilized. CN104120351B provides a method for preparing antibacterial stainless steel by using the tailings after depleting copper smelting slag in an electric furnace. After the copper smelting slag is depleted in an electric furnace to recover copper, it is then subjected to oxidation desulfurization-melting reduction-iron water purification, tempering and other processes to prepare antibacterial stainless steel. In this method, the copper content in the tailings after depletion in an electric furnace is low. If the copper content required for antibacterial stainless steel is to be obtained, a certain amount of copper needs to be added in the tempering process. In addition, since the copper-containing raw material needs to be oxidized and desulfurized, FeO in the copper slag is overoxidized to Fe2O3, thereby greatly increasing the liquid phase temperature of the copper slag, and a large amount of additives must be added to reduce the melting point of the copper slag and consume a large amount of reducing agent deoxidation. CN102952952B proposes oxidative desulfurization-natural gas injection reduction-gradient cooling to obtain two products, copper-rich ferroalloy and iron. This method uses pure oxygen for desulfurization and natural gas for reduction, which is costly and has low product purity, and has limited direct application. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing rare earth antibacterial stainless steel using copper smelting slag and rare earth antibacterial stainless steel, which can improve the shortcomings of using copper depleted tailings to prepare antibacterial stainless steel, such as the need for oxidative desulfurization of copper slag, large slag volume, low copper content in copper-iron alloy, and low copper slag utilization rate.
[0006] In a first aspect, the present invention provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag, using the following technical scheme:
[0007] A method for preparing rare earth antibacterial stainless steel using copper smelting slag, specifically comprising the following steps:
[0008] S1. Deep reduction: placing the undepleted high-temperature molten copper smelting slag discharged during the copper smelting process in a reduction furnace, adding a reducing agent and an additive for deep reduction to form a copper-iron alloy;
[0009] S2. Deep desulfurization: Pre-desulfurization agent and deep desulfurization agent are added to the molten copper-iron alloy to desulfurize the copper-iron alloy;
[0010] S3. Smelting, rolling, and heat treatment: The copper-iron alloy after desulfurization is smelted, and tempered during the smelting process to obtain rare earth antibacterial stainless steel water, which is then cast to form a steel billet. The steel billet is heat treated after rolling to prepare rare earth antibacterial stainless steel.
[0011] Optionally, in step S1, the copper content in the copper smelting slag is 2wt% to 7wt%.
[0012] Optionally, in step S1, the reducing agent is one or more of coke, coal powder, and graphite, and the mass ratio of the reducing agent to the copper smelting slag is 0.1-0.2:1.
[0013] Optionally, in step S1, the auxiliary agent is CaO, and the amount of the auxiliary agent added is calculated based on the binary basicity of the copper smelting slag, and the basicity is between 0.1 and 1.
[0014] Optionally, in step S1, the temperature of deep reduction is 1300-1500°C.
[0015] Optionally, in step S2, the pre-desulfurizer is graphite, the deep desulfurizer is at least one of CaO and MgO, or the deep desulfurizer is a mixture of at least one of CaO and MgO and at least one of Al2O3 and SiO2.
[0016] Optionally, in step S2, the mass ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is 0-0.2:0-0.6:1, wherein the mass ratio of the pre-desulfurizer and the deep desulfurizer is not zero.
[0017] Optionally, in step S2, the temperature of deep desulfurization is 1450-1550°C.
[0018] Optionally, in step S3, the composition of the rare earth antibacterial stainless steel water is Ni: 6.0-10.5%, Cr: 16.0-19.5%, Cu: 2.5-4.0%, Re: 0.4-0.8%, C≤0.03%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, N≤0.2%, in mass percentage, and the remainder is Fe.
[0019] In a second aspect, the present invention provides a rare earth antibacterial stainless steel, which is prepared by the aforementioned method of preparing rare earth antibacterial stainless steel using copper smelting slag. Trace amounts of rare earth are added in the form of rare earth iron alloy to increase the strength and antibacterial properties of the steel.
[0020] In summary, the present invention has at least one of the following beneficial effects:
[0021] 1. The present invention provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag, which can obtain a copper-iron alloy with a high copper content. Compared with using depleted copper slag as a raw material, it is not necessary to add metallic copper in the refining and modulation process. By optimizing the deep desulfurization process, the oxidative desulfurization process of the copper smelting slag is cancelled, and the copper-iron alloy is desulfurized instead, thereby avoiding the oxidative desulfurization of the copper smelting slag, which causes FeO in the copper smelting slag to peroxidize to Fe2O3, causing the liquid phase temperature of the copper smelting slag to rise sharply, so that the copper smelting slag can be reduced under low alkalinity conditions and low reduction temperatures, effectively reducing the amount of additives required in the reduction process.
[0022] 2. The present invention provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag. The deep desulfurization process adopts a two-step method. Since the saturated sulfur content of the deep desulfurizer is limited, excess graphite is first added to pre-desulfurize the alloy to effectively reduce the sulfur content in the copper-iron alloy. Then, a mixture of CaO, MgO or Al2O3, SiO2 as the main components is added as a deep desulfurizer. This can prevent the sulfur content in the deep desulfurizer from reaching saturation too early and affecting the desulfurization effect. In addition, the amount of the deep desulfurizer used is greatly reduced, and the deep desulfurizer can also synergize with excess graphite to further improve the desulfurization effect.
[0023] 3. The rare earth antibacterial stainless steel provided by the present invention is prepared by the aforementioned method, has low preparation cost and stable performance, and meets the requirements of the industry standard YB / T 4171-2020 "Copper-containing antibacterial stainless steel". DETAILED DESCRIPTION
[0024] The present invention provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag and rare earth antibacterial stainless steel. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] Copper smelting slag is produced in the copper smelting process. The copper smelting slag needs to be high-temperature depleted or flotation depleted to recover copper matte before it can be discarded or piled up. In the related technology, the tailings after the copper smelting slag is depleted are used to prepare antibacterial stainless steel. On the contrary, it is necessary to add a certain amount of copper in the steelmaking tempering process to meet the composition requirements of the antibacterial stainless steel. In addition, since the copper-containing raw materials need to be oxidized and desulfurized, the FeO in the copper slag is overoxidized to Fe2O3, which greatly increases the liquid phase temperature of the copper slag. A large amount of additives must be added to lower the melting point of the copper slag and a large amount of reducing agents are consumed for deoxidation. After long-term experimental research, the applicant found that undepleted copper smelting slag contains 2%-7% copper and 30%-40% iron. The undepleted high-temperature molten copper smelting slag discharged during the copper smelting process is first reduced to prepare a copper-iron alloy, and then deeply desulfurized. Combined with a specific two-step desulfurization process, a pre-desulfurizer and a deep desulfurizer are added successively to desulfurize the copper-iron alloy. The copper in the copper smelting slag can be directly reduced to the copper-iron alloy to the greatest extent, which omits the process of copper smelting slag depletion and copper recovery and the step of additional copper addition in the tempering process, and avoids the substantial increase in the liquid phase temperature of the copper slag caused by oxidative desulfurization. The copper smelting slag can be reduced under low alkalinity and low reduction temperature conditions, effectively reducing the amount of additives required in the reduction process.
[0026] The present invention provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag, which specifically comprises the following steps:
[0027] S1. Deep reduction: placing the undepleted high-temperature molten copper smelting slag discharged during the copper smelting process in a reduction furnace, adding a reducing agent and an additive for deep reduction to form a copper-iron alloy;
[0028] S2. Deep desulfurization: Pre-desulfurization agent and deep desulfurization agent are added to the molten copper-iron alloy to desulfurize the copper-iron alloy;
[0029] S3. Smelting, rolling, and heat treatment: The copper-iron alloy after desulfurization is smelted, and tempered during the smelting process to obtain rare earth antibacterial stainless steel water, which is then cast to form a steel billet. The steel billet is heat treated after rolling to prepare rare earth antibacterial stainless steel.
[0030] Specifically, in step S1, the copper content in the copper smelting slag is 2wt% to 7wt%, the reducing agent is one or more of coke, coal powder, and graphite, the auxiliary agent is CaO, and the reduction temperature is 1300 to 1500°C, preferably 1300 to 1400°C. The process of deep reduction is: (Cu) + (Fe) + (O) + C → [Cu] + [Fe] + CO↑, where () represents in the slag and [] represents in the alloy. The amount of the auxiliary agent CaO added is calculated based on the binary basicity (CaO / SiO2 mass ratio) of the copper smelting slag, and the basicity is between 0.1 and 1, preferably 0.4 to 0.6. The mass ratio of the reducing agent to the copper smelting slag is 0.1 to 0.2:1, preferably 0.14 to 0.16:1.
[0031] In step S2, the pre-desulfurizer is graphite, the deep desulfurizer is at least one of CaO and MgO, or the deep desulfurizer is a mixture of at least one of CaO and MgO and at least one of Al2O3 and SiO2. The deep desulfurization temperature is 1450-1550°C, preferably 1450-1500°C. The mass ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is 0-0.2:0-0.6:1, wherein the pre-desulfurizer and the deep desulfurizer are not 0, and the mass ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is preferably 0.1-0.2:0.2-0.6:1, and further preferably 0.15-0.2:0.3-0.4:1. The time for pre-desulfurization is 10min-30h, and the time for deep desulfurization is 10min-30h, which is adjusted according to the effect of desulfurization.
[0032] In step S3, the copper-iron alloy after desulfurization is smelted, and Ni, Cr, and Re are added during the smelting process for quenching and tempering to obtain rare earth antibacterial stainless steel water, the composition of the molten steel is Ni: 6.0-10.5%, Cr: 16.0-19.5%, Cu: 2.5-4.0%, Re: 0.4-0.8%, C≤0.03%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, N≤0.2%, in mass percentage, and the balance is Fe. After the molten steel is poured, it is rolled and heat-treated, so that the Cu precipitate phase that can produce a good antibacterial effect is evenly dispersed in the stainless steel matrix, and rare earth antibacterial stainless steel is obtained.
[0033] The present invention will be further described below by means of specific examples.
[0034] Example 1
[0035] This embodiment provides a method for preparing rare earth antibacterial stainless steel using copper smelting slag, and the preparation method includes the following preparation steps:
[0036] S1. Deep reduction: The undepleted high-temperature molten copper smelting slag discharged during the copper smelting process is placed in a reduction furnace. The composition of the copper smelting slag is: TFe 35.5%, TCu 4.5%, CaO 2.87%, SiO218.17%, MgO 2.63%, Al2O31.98%, S 1.09%. Under the condition of temperature of 1350℃, reducing agent graphite and auxiliary agent CaO are added for deep reduction to form copper-iron alloy. Among them, the amount of auxiliary agent CaO added is determined according to the basicity of the copper smelting slag, the basicity R = ω(CaO) / ω(SiO2), and the basicity is controlled to be 0.43, wherein ω(CaO) represents the mass fraction of CaO in the copper smelting slag, and ω(SiO2) represents the mass fraction of SiO2 in the copper smelting slag; the amount of reducing agent added is added according to the mass ratio of reducing agent graphite to copper smelting slag of 0.14:1; after reaction reduction, high-temperature copper-iron alloy and tailings are obtained, and the composition of the tailings is detected. The copper and iron contents in the tailings are reduced to 0.07% and 2.5%, respectively, in mass percentage.
[0037] S2. Deep desulfurization: Pre-desulfurization agent and deep desulfurization agent are added to the molten copper-iron alloy successively to desulfurize the copper-iron alloy. The pre-desulfurization is 30 minutes and the desulfurization temperature is 1500℃. The pre-desulfurization agent is graphite, and the deep desulfurization agent is CaO and Al2O3. The mass ratio of CaO to Al2O3 is 2:1, and the mass ratio of pre-desulfurization agent, deep desulfurization agent and copper-iron alloy is 0.15:0.3:1. The sulfur content in the copper-iron alloy is detected. The sulfur content in the copper-iron alloy after pre-desulfurization is 1.3%, and the sulfur content in the copper-iron alloy after deep desulfurization is 0.02%, calculated by mass percentage.
[0038] S3. Smelting, rolling and heat treatment: The desulfurized copper-iron alloy is sent to the steelmaking process for smelting. Ni, Cr and Re are added during the smelting process for tempering to obtain rare earth antibacterial stainless steel water. The composition of the molten steel is C≤0.03%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, Ni: 6%, Cr: 19.5%, Cu: 4%, N≤0.2%, Re: 0.5%, calculated by mass percentage, and the balance is Fe. It is then cast into a steel billet and then heat treated to prepare rare earth antibacterial stainless steel, which meets the requirements of the industry standard YB / T 4171-2020 "Copper-containing antibacterial stainless steel".
[0039] Example 2
[0040] The difference between Example 2 and Example 1 is that in step S1 of Example 2, the temperature of deep reduction is 1450°C. The composition of the tailings in step S1 was detected, and the copper and iron contents in the tailings were reduced to 0.45% and 1.7%, respectively, in mass percentage. The sulfur content in the copper-iron alloy after deep desulfurization in step S2 was detected. The sulfur content in the copper-iron alloy after pre-desulfurization was 1.3%, and the sulfur content in the copper-iron alloy after deep desulfurization was 0.02%, in mass percentage. The rare earth antibacterial stainless steel prepared in step S3 meets the requirements of the industry standard YB / T 4171-2020 "Copper-containing antibacterial stainless steel".
[0041] Example 3
[0042] The difference between Example 3 and Example 1 is that in step S1 of Example 3, the amount of reducing agent added is according to the mass ratio of reducing agent graphite to copper smelting slag of 0.13:1. The composition of the tailings in step S1 was detected, and the copper and iron contents in the tailings were reduced to 0.11% and 5.4%, respectively, in mass percentage. The sulfur content in the copper-iron alloy after deep desulfurization in step S2 was detected. The sulfur content in the copper-iron alloy after pre-desulfurization was 1.3%, and the sulfur content in the copper-iron alloy after deep desulfurization was 0.02%, in mass percentage. Step S3 prepares rare earth antibacterial stainless steel, which meets the requirements of industry standard YB / T 4171-2020 "Copper-containing antibacterial stainless steel".
[0043] Example 4
[0044] The difference between Example 4 and Example 1 is that in step S2 of Example 4, the mass ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is 0.05: 0.6: 1. The sulfur content in the copper-iron alloy after deep desulfurization in step S2 is detected. The sulfur content in the copper-iron alloy after pre-desulfurization is 1.74%, and the sulfur content after deep desulfurization is 0.46%, calculated in mass percentage.
[0045] Example 5
[0046] The difference between Example 5 and Example 1 is that in step S2 of Example 5, the desulfurization temperature is 1550°C. The sulfur content in the copper-iron alloy after deep desulfurization in step S2 is detected. The sulfur content in the copper-iron alloy after pre-desulfurization is 2.2%, and the sulfur content after deep desulfurization is 0.025%, measured in mass percentage. The rare earth antibacterial stainless steel prepared in step S3 meets the requirements of the industry standard YB / T 4171-2020 "Copper-containing antibacterial stainless steel".
[0047] Example 6
[0048] The difference between Example 6 and Example 1 is that in step S2 of Example 6, the ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is 0.15: 0.2: 1. The sulfur content in the copper-iron alloy after deep desulfurization in step S2 is detected. The sulfur content in the alloy after pre-desulfurization is 1.3%, and the sulfur content after deep desulfurization is 0.15%, calculated in mass percentage.
[0049] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing rare earth antibacterial stainless steel using copper smelting slag, characterized in that: The specific steps include: S1. Deep reduction: placing the undepleted high-temperature molten copper smelting slag discharged during the copper smelting process in a reduction furnace, adding a reducing agent and an additive for deep reduction to form a copper-iron alloy; S2. Deep desulfurization: Pre-desulfurization agent and deep desulfurization agent are added to the molten copper-iron alloy to desulfurize the copper-iron alloy; S3. Smelting, rolling and heat treatment: the copper-iron alloy after desulfurization is smelted, and the rare earth antibacterial stainless steel water is obtained by quenching and tempering during the smelting process, and then cast to form a steel billet, and the steel billet is heat treated after rolling to prepare rare earth antibacterial stainless steel; In step S1, the copper content in the copper smelting slag is 2wt%~7wt%; In step S3, the composition of the rare earth antibacterial stainless steel water is Ni: 6.0~10.5%, Cr: 16.0~19.5%, Cu: 2.5~4.0%, Re: 0.4~0.8%, C≤0.03%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, N≤0.2%, in mass percentage, and the remainder is Fe.
2. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S1, the reducing agent is one or more of coke, coal powder, and graphite, and the mass ratio of the reducing agent to the copper smelting slag is 0.1-0.2:
1.
3. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S1, the auxiliary agent is CaO, and the amount of the auxiliary agent added is calculated based on the binary basicity of the copper smelting slag, and the basicity is between 0.1 and 1.
4. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S1, the temperature of deep reduction is 1300~1500°C.
5. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S2, the pre-desulfurizer is graphite, the deep desulfurizer is at least one of CaO and MgO, or the deep desulfurizer is a mixture of at least one of CaO and MgO and at least one of Al2O3 and SiO2.
6. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S2, the mass ratio of the pre-desulfurizer, the deep desulfurizer and the copper-iron alloy is 0-0.2:0-0.6:1, wherein the mass ratio of the pre-desulfurizer and the deep desulfurizer is not zero.
7. The method for preparing rare earth antibacterial stainless steel using copper smelting slag according to claim 1, characterized in that: In step S2, the temperature of deep desulfurization is 1450-1550°C.
8. A rare earth antibacterial stainless steel prepared by the method for preparing rare earth antibacterial stainless steel using copper smelting slag according to any one of claims 1 to 7.