A catalyst for preparing low-carbon alkanes and its preparation and application
The preparation of copper-ferroalloy catalysts through physical sputtering method solves the problem of difficult-to-understand the coordinated catalytic mechanism of active components in the carbon dioxide hydrogenation reaction, and achieves low-cost and environmentally friendly catalyst preparation, improves the selectivity of alkanes and is suitable for industrial production.
Patent Information
- Application Number
- CN202210037338.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-01-13
AI Technical Summary
In the prior art, it is difficult to clearly understand the synergistic catalytic mechanism between active components in the carbon dioxide hydrogenation reaction, and traditional catalyst preparation methods have problems of environmental pollution and high energy consumption.
In the Ar ion bombardment state, the copper atoms and iron atoms are fully mixed to form a copper ferroalloy catalyst. A high specific surface area oxide material is used as a support to avoid high-temperature calcination and nitrate solution, and a CuFe catalyst is prepared.
It realizes low-cost and environmentally friendly catalyst preparation. The catalyst has high selectivity and stability, is suitable for large-scale industrial production, and has high alkane selectivity, avoiding the sintering and oxidation problems of metal components in traditional methods.
Smart Images

Figure CN116474778B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst for carbon dioxide hydrogenation reaction and its application field, and in particular to an alloy catalyst for preparing low-carbon alkanes (C1-C4) by carbon dioxide hydrogenation and its application. Background Art
[0002] The emission of greenhouse gases such as carbon dioxide (CO2) has increased year by year, causing many environmental problems including ocean acidification and greenhouse effect. Currently, cheap metals such as copper-based, iron-based, and cobalt-based are widely used in catalysts and are widely used in the preparation of low-carbon olefins, high-carbon alcohols, and high-carbon hydrocarbons. However, it is difficult to clearly understand the synergistic catalytic mechanism between active components.
[0003] It is generally believed that copper-based catalysts are mainly active sites for methanol synthesis and reverse water gas shift. For example, Cu-ZnO-Al2O3 is a widely used industrial catalyst with low price and high activity. In addition, other series of copper-based catalysts such as Cu-ZnO-ZrO2 have also enriched the application of such catalysts.
[0004] Iron-based and cobalt-based catalysts are used in the CO2 hydrogenation reaction to synthesize high-carbon hydrocarbons. x C y 、CoC x It is considered as the active site for promoting CC chain growth. Adding alkali metal additives will further enhance the chain growth ability and further improve the selectivity of long-chain substances.
[0005] According to the research results published so far, the CO2 product of Cu / ZnO catalyst is methanol, but after adding Fe component, the main product will become olefin. This is true for both impregnation and precipitation methods. How to change the intimacy by adjusting the introduction method of metal and thus change the product selectivity is a research difficulty. Summary of the invention
[0006] In view of the above problems in the prior art, the purpose of the present invention is to provide a simple, low-cost, easy-to-use copper-iron alloy catalyst for use in the carbon dioxide hydrogenation reaction.
[0007] The present invention adopts a physical sputtering method. Under the state of Ar ion bombardment, copper atoms and iron atoms are fully mixed to form an alloy on the surface of the carrier. In this state, the copper and iron components have a very close relationship with each other, which makes the catalyst have a unique catalytic effect.
[0008] The catalyst of the present invention uses an oxide material with a high specific surface area as a carrier, copper and iron as active components, and is prepared in one step by a physical sputtering method.
[0009] The physical sputtering method for preparing CuFe catalyst comprises the following steps: (1) using a magnetron sputtering device to prepare the catalyst, cleaning the surface of the target material before preparation, bombarding the copper and iron targets (mass purity of more than 99.9%) with Ar ions generated by two plasma generators for 1-30 minutes, preferably 10-30 minutes; (2) placing the carrier powder in a circular rotating barrel, and evacuating the vacuum chamber to a pressure of 9.9×10 -4 Pa or less, preferably 9.9×10 -6 -9.9×10 -4 Pa; (3) Ar (volume purity of more than 99.9%) is introduced into the vacuum chamber at a flow rate of 10-50 ml / min, preferably 12-30 ml / min, and the pressure of the vacuum chamber is maintained at 0.5-3.0 Pa, preferably 0.5-1.5 Pa; (4) the power of the two plasma generators is adjusted to 100-400 W respectively, the ion generator where the copper target is located is preferably 100-200 W, and the ion generator where the iron target is located is preferably 250-350 W; the barrel speed is increased to 1-20 rpm, preferably 5-10 rpm; the Cu and Fe metal nanoparticles generated by the bombardment of the target by Ar ions can be uniformly deposited on the surface of the carrier; (5) After the sputtering is completed, an O2 / Ar mixed gas is introduced into the vacuum chamber for passivation for 30 minutes, and Ar is continued to be introduced until the pressure reaches normal pressure, wherein the volume concentration of O2 is 0.5-5%, preferably 1-3%.
[0010] The mass content of the active component copper in the prepared catalyst is 10-30%, preferably 15-25%; the mass content of iron is 3-8%, preferably 3-5%, and the rest is a carrier. The carrier can be one or a mixture of two or more of SiO2, Al2O3, CeO2, ZrO2, MgO, Fe3O4, etc., with a high specific surface area (50-200m 2 / g) of oxide material. The catalyst prepared by this method does not need to be calcined, and the species on the fresh catalyst is a zero-valent metal, the reduction temperature is low, and it is not easily oxidized during the reaction.
[0011] The hydrogenation reaction conditions for the catalyst are as follows: the raw materials are hydrogen and carbon dioxide, the molar ratio of the two is 1-10, preferably 3-5; the reaction temperature is 200-400°C, preferably 250-350°C; the reaction pressure is 1.0-10.0MPa, preferably 2.0-4.0MPa; the mass space velocity of the raw gas is 3000-10000ml / (g cat h), preferably 5000-8000ml / (g cat h).
[0012] The advantages of the present invention are: (1) the catalyst is prepared in one step by a physical sputtering method, avoiding a series of steps of using nitrate solution and high-temperature roasting in the general preparation method, effectively preventing environmental pollution and excessive energy consumption; (2) the alloy nanoparticles are evenly dispersed (TEM), the particle radius is small (at 5-7nm), the metal utilization rate is high, and it is not easy to sinter and aggregate; (3) Cu and Fe metals exist in the form of alloy (FeCu4), which is stable under reducing atmosphere and reaction conditions. Under this combination mode, there is a special electronic effect in the Cu-Fe-carrier, resulting in a higher selectivity for alkanes. On the contrary, the use of impregnation method or the addition of alkali additives will break the strong interaction between Cu and Fe, resulting in an increase in the selectivity of olefins; (4) the preparation of the catalyst is less affected by environmental and human factors, no pollutants are discharged, and it is suitable for large-scale industrial production of hydrogenation to produce chemicals. The use of this technology to prepare the catalyst and use it in the reaction of hydrogenating carbon dioxide to produce alkanes has not been reported, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Table 1 shows the catalyst reaction performances of Example 1, Example 8, Comparative Example 1, and Comparative Example 2.
[0014] Figure 1 These are the XRD diffraction patterns of the catalysts of Example 8 (sp-Cu15Fe5Zn), Comparative Example 1 (im-Cu15Fe5Zn), and Comparative Example 2 (sp-Cu15Fe5ZnK) before and after the reaction.
[0015] Figure 2 This is the TEM image of Example 8 (sp-Cu15Fe5Zn). Specific implementation methods
[0016] The technical details of the present invention are described in detail by the following examples. It should be noted that the examples are only used to further illustrate the technical features of the present invention, rather than to limit the present invention.
[0017] Example 1
[0018] The catalyst was prepared using a commercial magnetron sputtering device with two target heads (one plasma generator on each target head) (manufacturer: Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences, the same below). The copper target and the iron target were respectively mounted on the two target heads, and two plasma generators were used to generate Ar ions to pre-bombard the high-purity copper target (mass purity of 99.99%) and the iron target (mass purity of 99.9%) for 30 minutes, and then 10g of ZnO carrier (specific surface area 70m 2 / g) powder was placed in a cylindrical rotating drum, and the vacuum chamber was evacuated to a pressure of 9.9×10 -4Pa, high-purity Ar gas (volume purity 99.95%) was introduced at a flow rate of 20ml / min, and the pressure was maintained until it reached 0.5Pa. The power of the iron target ion generator was adjusted to 300W, the power of the copper target was adjusted to 200W, and the rotating drum speed was increased to 5rpm, so that the nano-metal particles produced by Ar ion bombardment of the target material (TEM electron microscope observed that the copper-iron alloy nanoparticle size was 5-7nm) were uniformly deposited on the carrier surface, and sputtered for 3 hours. After the sputtering, the vacuum chamber was passed through a 1% volume content O2 / Ar mixed gas passivation for 30min, and then Ar was introduced to restore to normal pressure. After testing, a catalyst with a Cu mass loading of 25% and an iron loading of 5% was obtained, which was recorded as sp-Cu25Fe5Zn. 50%-70% of Fe exists in the form of active component FeCu4 (the rest is Cu and Fe nanoparticles existing alone), and Cu-Fe metal bonds can be observed by EXAFS analysis.
[0019] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and pure H2 was used for reduction at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced, with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 35.8%, and the carbon monoxide selectivity was 12.1%. In addition to carbon monoxide, all other products were organic products. Among the organic products, the selectivity of alkanes was 77.5%, of which C1-C4 alkanes accounted for 50.2%; olefins (C4-C 14 ) selectivity is 18.5%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 4.0%.
[0020] Example 2
[0021] The 0.5 gsp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and reduced with pure H2 at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced, with a H2 / CO2 molar ratio of 3. The reaction temperature was 310°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 23.1%, and the carbon monoxide selectivity was 18.5%. In addition to carbon monoxide, the products were organic. Among the organic products, the selectivity of alkanes was 80.1%, of which C1-C4 alkanes accounted for 56.4%; olefins (C4-C 14 ) selectivity is 14.7%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 5.2%.
[0022] Example 3
[0023] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and reduced with pure H2 at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced, with a H2 / CO2 molar ratio of 3. The reaction temperature was 370°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 43.1%, and the carbon monoxide selectivity was 10.8%. In addition to carbon monoxide, the products were organic. Among the organic products, the selectivity of alkanes was 77%, of which C1-C4 alkanes accounted for 50.2%; olefins (C4-C 14 ) selectivity is 20.9%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 2.1%.
[0024] Example 4
[0025] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and pure H2 was used for reduction at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced, with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 2 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 32.6%, and the carbon monoxide selectivity was 23.1%. In addition to carbon monoxide, the products were organic. Among the organic products, the selectivity of alkanes was 68.8%, of which C1-C4 alkanes accounted for 47.2%; olefins (C3-C 14 ) selectivity is 30.4%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 0.8%.
[0026] Example 5
[0027] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and pure H2 was used for reduction at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced, with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 4 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 35.8%, and the carbon monoxide selectivity was 16.6%. In addition to carbon monoxide, the products were organic. Among the organic products, the selectivity of alkanes was 66.2%, of which C1-C4 alkanes accounted for 44%; olefins (C3-C 14 ) selectivity is 30.5%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 3.3%.
[0028] Example 6
[0029] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and reduced with pure H2 at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 4800 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 33.6%, and the carbon monoxide selectivity was 18.7%. In addition to carbon monoxide, all other products were organic products. Among the organic products, the selectivity of alkanes was 70.2%, of which C1-C4 alkanes accounted for 50%; olefins (C3-C 14 ) selectivity is 25.2%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 4.6%.
[0030] Example 7
[0031] 0.5 g of sp-Cu25Fe5Zn catalyst prepared in Example 1 was loaded into a fixed bed reactor, and reduced with pure H2 at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 9600 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 28.7%, and the carbon monoxide selectivity was 27.9%. In addition to carbon monoxide, all other products were organic products. Among the organic products, the selectivity of alkanes was 68.1%, of which C1-C4 alkanes accounted for 51.9%; olefins (C3-C 10 ) selectivity is 27.6%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 4.3%.
[0032] Example 8
[0033] The catalyst was prepared using a commercial magnetron sputtering device with two target heads (one plasma generator on each target head) (manufacturer: Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences). The copper target and the iron target were respectively mounted on the two target heads, and two plasma generators were used to generate Ar ions to pre-bombard the high-purity copper target (mass purity of 99.99%) and the iron target (mass purity of 99.9%) for 30 minutes, and then 10g of ZnO carrier (specific surface area 70m 2 / g) The powder is placed in a cylindrical rotating drum, and the vacuum chamber is evacuated to a pressure of 9.9×10 -4Pa, high-purity Ar gas (volume purity 99.95%) was introduced at a flow rate of 20ml / min, and the pressure was maintained until it reached 0.5Pa. The power of the iron target ion generator was adjusted to 300W, the power of the copper target was adjusted to 100W, and the rotating drum speed was increased to 5rpm, so that the nano-metal particles produced by Ar ion bombardment of the target material (TEM electron microscope observed that the copper-iron alloy nanoparticle size was 5-7nm) were uniformly deposited on the carrier surface, and sputtered for 3 hours. After the sputtering was completed, a 1% volume content O2 / Ar mixed gas was introduced into the vacuum chamber for passivation for 30min, and then Ar was introduced to restore to normal pressure. After testing, a catalyst with a Cu mass loading of 15% and an iron loading of 5% was obtained, which was recorded as sp-Cu15Fe5Zn. 50%-70% of Fe exists in the form of active component FeCu4 (the rest is Cu and Fe nanoparticles existing alone), and Cu-Fe metal bonds can be observed by EXAFS analysis.
[0034] 0.5 g of sp-Cu15Fe5 / ZnO catalyst prepared in Example 8 was loaded into a fixed bed reactor and reduced with pure H2 at 250°C for 8 h under normal pressure. A raw gas H2 / CO2 mixed gas was introduced with a H2 / CO2 molar ratio of 3. The reaction temperature was 340°C, the pressure was 3 MPa, and the mass space velocity of the raw gas was 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 33.4%, and the carbon monoxide selectivity was 18.0%. In addition to carbon monoxide, all other products were organic products. Among the organic products, the selectivity of alkanes was 76.5%, of which C1-C4 alkanes accounted for 53.9%; olefins (C3-C 10 ) selectivity is 19.4%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 4.1%.
[0035] Comparative Example 1
[0036] Preparation of impregnation catalyst: 4.51gFe(NO3)3·9H2O and 7.09gCu(NO3)2·3H2O were dissolved in 12ml of deionized water, then dripped into 10g ZnO powder drop by drop with a dropper, stirred evenly, ultrasonicated for 30min, and impregnated overnight. Then put it in an oven at 80℃ for 6h to dry, and then transfer the sample into a muffle furnace and roast it at 400℃ for 4h. XRF characterization showed that the catalyst with a mass loading of 15% Cu and a mass loading of 5% iron was obtained, which was recorded as im-Cu15Fe5Zn. XRD characterization found that the Cu and Fe components existed in the form of oxides, and no alloy was formed during the preparation process.
[0037] 0.5 g of the im-Cu15Fe5Zn catalyst prepared in Comparative Example 1 was loaded into a fixed bed reactor. The catalyst was reduced with pure hydrogen for 8 h at 350° C. under normal pressure. A raw gas H2 / CO2 mixed gas was introduced with a H2 / CO2 molar ratio of 3, a reaction temperature of 340° C., a pressure of 3 MPa, and a mass space velocity of 7200 ml / (g cat h), and data were collected after 8 h of reaction. The carbon dioxide conversion rate was 31.3%, the carbon monoxide selectivity was 22.8%, and all products except carbon monoxide were organic products. Among the organic products, the selectivity of alkanes was 27.5%, of which C1-C4 alkanes accounted for 21.6%; olefins (C2-C 10 ) selectivity is 63.5%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 9%.
[0038] Comparative Example 2
[0039] Based on the catalyst obtained in Example 8, anhydrous K2CO3 with a final mass fraction of 0.5% was added to the catalyst obtained in Example 8 by grinding to obtain sp-Cu15Fe5ZnK. XRD characterization found that the FeCu diffraction peak shifted to the position of metallic copper, indicating the decomposition of the alloy during the reaction.
[0040] 0.5 g of the sp-Cu15Fe5ZnK catalyst prepared in Comparative Example 2 was loaded into a fixed bed reactor. The catalyst was reduced with pure hydrogen for 8 h at normal pressure and a reduction temperature of 250° C. A raw gas H2 / CO2 mixed gas was introduced with a H2 / CO2 molar ratio of 3, a reaction temperature of 340° C., a pressure of 3 MPa, and a mass space velocity of 7200 ml / (g cat h), and the data was collected after 8 h of reaction. The carbon dioxide conversion rate was 34.8%, the carbon monoxide selectivity was 21.0%, and all products except carbon monoxide were organic products. Among the organic products, the selectivity of alkanes was 26.1%, of which C1-C4 alkanes accounted for 18.9%; olefins (C2-C 10 ) selectivity is 61.7%, and the selectivity of alcohols (CH3OH, CH3CH2OH) is 12.2%.
[0041] Example results: From the above results, under the same reaction conditions, the selectivity of sp-Cu15Fe5Zn alkanes prepared by physical sputtering in one step is higher, which is due to the strong interaction between metals in FeCu4 alloy. It can be observed from the XRD spectrum that the sp-Cu15Fe5Zn catalyst prepared by magnetron sputtering technology has a very obvious alloy peak of FeCu4 at 43.3° in the fresh state without use, while the metal components of im-Cu15Fe5Zn prepared by impregnation method are all in the form of oxides; after 8h of reaction, sp-Cu15Fe5Zn has a very strong alloy peak, while im-Cu15Fe5Zn has metal Cu (43.2°) and Fe x C, while the diffraction peak of sp-Cu15Fe5ZnK is between the two, indicating that under the influence of K additive, the alloy decomposes and the interaction between copper and iron weakens, resulting in less alkane content and higher olefin content in the product. This preparation method is less affected by experimental operating conditions, but is limited by the output of the sputtering device.
[0042]
[0043] Note: 1. Selectivity refers to the proportion of each component in the total organic product after CO removal.
[0044] 2. The data in brackets are the selectivity for low-carbon alkanes (C1-C4).
[0045] Table 1. Catalyst reaction performance of Example 1 (sp-Cu25Fe5Zn), Example 8 (sp-Cu15Fe5Zn), Comparative Example 1 (im-CuFeZn), and Comparative Example 2 (sp-Cu15Fe5ZnK).
[0046] Compared with the traditional precipitation method and impregnation method, the advantages of this invention are mainly reflected in: (1) it does not require the use of nitrate as a metal source and high-temperature roasting steps, thus avoiding environmental pollution and the problem of easy sintering of metal components during the preparation process; (2) the active metal has the characteristics of uniform particle size, high dispersion and easy reduction; (3) a unique FeCu4 alloy active phase is formed during the preparation process, which can be used for the reaction of hydrogenating carbon dioxide to produce low-carbon alkanes.
Claims
1. Application of a catalyst for preparing light alkanes, Features: The catalyst is used in the reaction of hydrogenating carbon dioxide to produce light alkanes; The catalyst is used in a fixed bed reactor, and the hydrogenation reaction conditions are: the raw materials are hydrogen and carbon dioxide, the molar ratio of the two is 1-10, the reaction temperature is 200-400 ℃; the reaction pressure is 1.0-10.0 MPa; the mass space velocity of the raw gas is 3000-10000 mL / (g cat h); The catalyst is a supported catalyst, which uses metal oxide materials as carriers. The carrier is SiO 2 、Al 2 O 3 、CeO 2 、ZrO 2 ,MgO,Fe 3 O 4 One or more of FeCu 4 The alloy is an active component, and the active component is prepared on a carrier in one step by a physical sputtering method. The copper and iron species on the carrier of the prepared catalyst are both zero-valent metals; the mass content of copper in the catalyst is 15-30%; the mass content of iron is 3-8%.
2. The use according to claim 1, Features: The hydrogenation reaction conditions are as follows: the raw materials are hydrogen and carbon dioxide, the molar ratio of the two is 3-5; the reaction temperature is 250-350°C; the reaction pressure is 2.0-4.0 MPa; the mass space velocity of the raw gas is 5000-8000 mL / g cat / h.
3. The use according to claim 1, Features: The mass content of copper in the catalyst is 15-25%; the mass content of iron is 3-5%, and the specific surface area of the carrier ranges from 50 to 200 m 2 / g.
4. The use according to claim 3, Features: The specific surface area of the carrier ranges from 50 to 80 m 2 / g.
5. The use according to claim 1, Features: The copper and iron-based catalysts prepared by physical sputtering do not require calcination treatment; the catalyst uses a material with a high specific surface area as a carrier; and the active components are stable during the reaction, and the copper-iron alloy nanoparticles do not sinter and aggregate, and are used for the reaction of hydrogenating carbon dioxide to prepare low-carbon alkanes.
6. The use according to claim 5, The following steps are involved: The catalyst is prepared by using a magnetron sputtering device, in which two target heads are arranged in a vacuum chamber, and each target head corresponds to a plasma generator; (1) Before preparation, the target surface is pre-cleaned: a copper target and an iron target are respectively installed on two target heads in a vacuum chamber, Ar gas is used as the working gas, and Ar ions generated by two plasma generators are used to bombard the copper and iron targets for 1-30 minutes respectively; the mass purity of the copper and iron targets is above 99.9%; (2) The carrier powder is placed in a rotating drum with a circular radial cross section and axially rotatable in the vacuum chamber of a magnetron sputtering device, and the vacuum chamber is evacuated to a pressure of 9.9× 10 -4 Below Pa; (3) Ar gas with a volume purity of more than 99.9% is introduced into the vacuum chamber at a flow rate of 10-50 mL / min, and the pressure of the vacuum chamber is maintained at 0.5-3.0 Pa; (4) The power of the two plasma generators is adjusted to 100-400 W respectively, and the rotating barrel speed is increased to 1-20 rpm, so that the copper and iron nanoparticles generated by the Ar ion bombardment of the target material are uniformly deposited on the surface of the carrier; sputtering for 2-6 hours; (5) After sputtering, O is introduced into the vacuum chamber. 2 / Ar mixed gas passivation for 30-60 minutes, then introduce Ar until the pressure reaches normal pressure, and open the magnetron sputtering vacuum chamber door; 2 O in Ar / Mixed Gas 2 The volume concentration is 0.5-5% to obtain the desired catalyst.
7. The use according to claim 6, Features: In step (1), Ar ions generated by two plasma generators are used to bombard the copper and iron targets for 10-30 minutes respectively; In step (2), the vacuum chamber is evacuated to a pressure of 9.9 × 10 -6 -9.9× 10 -4 Pa; In step (3), Ar gas with a volume purity of 99.9% or more is introduced into the vacuum chamber at a flow rate of 12-30 mL / min, and the pressure of the vacuum chamber is maintained at 0.5-1.5 Pa; In step (4), the power of the ion generator where the copper target is located is 100-200W, and the power of the ion generator where the iron target is located is 250-350W; the rotating barrel speed is increased to 5-10 rpm; the copper and iron nanoparticles generated by the Ar ion bombardment of the target material are uniformly deposited on the surface of the carrier; and the sputtering is performed for 2-6 hours; After the sputtering in step (4) is completed, O is introduced into the vacuum chamber. 2 / Ar mixed gas passivation for 20-30 minutes; then introduce Ar until the pressure reaches normal pressure, and open the magnetron sputtering vacuum chamber door; 2 O / Ar mixed gas 2 The volume concentration is 1-3%; the desired catalyst is obtained.
8. The use according to claim 1, Features: The catalyst needs to be heated to pure H at 250-340°C under normal pressure before the hydrogenation reaction. 2 Reduction 4-8h.
9. The use according to claim 8, Features: The catalyst needs to be heated to pure H at 250 °C under normal pressure before the hydrogenation reaction. 2 Reduction for 8 hours.
Citation Information
Patent Citations
Copper-based catalyst for preparing methyl glycolate and preparation and application thereof
CN110871071A
Method for preparing carbon-containing compound by electro-catalyzing carbon dioxide with copper alloy material
CN111074294A
Application of iron-based catalyst in synthesis of low-carbon olefin by carbon dioxide hydrogenation
CN112169815A
Preraring method for synthesis gas and hydrogen, and apparatus for the same