Method for preparing black conductive nano calcium carbonate by biogas slurry synchronous double decomposition coating method
Black conductive nano-calcium carbonate was prepared by a biogas slurry synchronous metathesis coating method. The nano-calcium carbonate crystal nuclei were coated with soluble humic acid, which solved the problems of complex and high cost of existing processes and achieved efficient and low-cost preparation of conductive nano-calcium carbonate, thus enhancing the antistatic and conductive properties of polymer materials.
Patent Information
- Application Number
- CN202310239259.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-03-13
AI Technical Summary
The existing asynchronous method for preparing black conductive nano-calcium carbonate is complex, costly, and the finished product is prone to agglomeration, which affects the quality uniformity of the conductive powder and cannot effectively solve the electrostatic problem of polymer materials.
Conductive nano-calcium carbonate was prepared in biogas slurry through a metathesis reaction using a simultaneous metathesis coating method. The nano-calcium carbonate crystal nuclei were coated with soluble humic acid organic matter to control the particle size and prevent agglomeration, thus forming black conductive nano-calcium carbonate.
This method enables efficient and low-cost preparation of conductive nano-calcium carbonate, solves the static electricity problem, enhances the toughness and conductivity of polymer materials, and possesses both antistatic and conductive functions, making it suitable for polymer materials such as plastics and rubber.
Smart Images

Figure CN116477652B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional material development, and in particular to a method for preparing black conductive nano calcium carbonate by a biogas slurry synchronous double decomposition coating method. Background Art
[0002] Plastics, rubber and other polymer materials, such as polyvinyl chloride (PVC), have good insulation properties and a resistance of up to 10 15 Ω or even higher, static charge accumulation occurs in certain use occasions, leading to static electricity hazards. For example, excessive static electricity accumulation may cause a fire when refueling a car, cause the vehicle to run at too high a temperature while driving, increase vehicle operating losses, shorten vehicle life, and even cause the vehicle to spontaneously combust. The tread rubber resistivity is less than 10 8 Ω·cm can smoothly conduct the static electricity generated during the driving of the car. Plastics, rubber and other polymer materials have high mechanical properties, good chemical corrosion resistance and flame retardancy, low price, and are used in industrial production. However, the surface of such polymer materials is very easy to accumulate static charge due to friction, spark discharge occurs, and causes the combustion and explosion of flammable gases, which limits its application in special fields such as coal mines, petroleum, chemicals, textiles, dangerous goods warehouses, electronics and wireless communications, and semiconductor industries. By filling conductive powder into such polymer materials to make the two compatible, such polymer materials can be developed from the production of plates, pipes, conveyor belts, equipment covers and other products to special fields.
[0003] Traditional conductive powders are divided into metal type, metal oxide type and carbon type. Conductive nano calcium carbonate, unlike traditional conductive powder, is a composite nano material with both filler and antistatic functions, that is, while adding nano calcium carbonate to solve the structural function of the material, it also solves the antistatic problem of the material. Compared with the step-by-step addition of nano materials to improve the structure and the addition of conductive powder to solve static electricity, conductive nano calcium carbonate powder is used as an antistatic agent material in the fields of plastics, rubber, etc. It not only gives plastics and rubber polymers antistatic properties, but also does not cause static electricity hazards in the use occasions. At the same time, the excellent performance of nano calcium carbonate itself can also enhance the toughness, tensile strength, thermal stability, etc. of plastics, rubber and other products. Due to the advantages of ultra-fine, large amount and good interface compatibility of conductive nano calcium carbonate, it can overcome the poor conductivity caused by ordinary antistatic agents due to large particle size, large particle spacing, poor dispersibility, poor interface compatibility, poor antistatic effect, antistatic agent precipitation causing antistatic failure and safety issues in use.
[0004] Although the excellent properties of conductive nano calcium carbonate are known, nano calcium carbonate itself is not conductive and cannot solve the problem of static electricity, so a special preparation process must be adopted. The currently reported preparation methods of conductive nano calcium carbonate all use nano calcium carbonate as a matrix and a composite conductive powder coated with an inorganic or organic conductive material. This coating method using nano calcium carbonate products as templates is called an asynchronous method for nano calcium carbonate production and conductive coating. However, the disadvantages of the existing asynchronous method for preparing black conductive nano calcium carbonate are that the production process is complicated, the product cost is high, and the finished nano calcium carbonate is easy to agglomerate during the coating process, which increases the particle size and affects the uniformity of the conductive powder quality.
[0005] The synchronous process of nano-calcium carbonate production and conductive coating, that is, synthesizing nano-calcium carbonate in an inorganic precursor solvent and coating it with a polymer at the same time, is synchronized with the double decomposition production process of nano-calcium carbonate. The advantages of this synchronous double decomposition and synchronous coating process are: 1) The double decomposition production process conditions are controllable, and the quality of the generated nano-calcium carbonate products is controllable, which is the core process of high-end nano-calcium carbonate at present; 2) The synchronous coating method can not only be used to produce conductive nano-calcium carbonate, but also is the basic process of high-end modified nano-calcium carbonate; 3) The presence of the coating polymer can effectively control the unlimited growth of the particle size of inorganic nanoparticles and prevent the agglomeration of nanoparticles, that is, it solves the problems of uneven dispersion and easy agglomeration of nanopowders in inorganic / organic composite materials in the existing asynchronous coating method.
[0006] The currently reported sodium carbonate and calcium chloride undergo double decomposition reaction in a mixed aqueous solution of polyvinyl pyrrolidone (PVP) and sodium dodecylbenzene sulfonate (SDBS) to prepare nano calcium carbonate, which can obtain spherical nano calcium carbonate with good dispersibility. So far, there has been no report on the use of biogas slurry to prepare black conductive nano calcium carbonate using the theory and method of synchronous double decomposition coating. This not only realizes the resource utilization of biogas slurry, but also realizes the high added value utilization of biogas slurry, filling the gap in the current preparation method and product of conductive nano calcium carbonate composite powder. Summary of the invention
[0007] In view of this, the present invention provides a method for preparing black conductive nano-calcium carbonate by a biogas slurry synchronous double decomposition coating method; using the biogas slurry produced in the production process of the biogas industry as a raw material, the biogas slurry synchronous double decomposition coating method is carried out to produce conductive nano-calcium carbonate. Biogas slurry is the product of anaerobic fermentation of organic waste. Because anaerobic fermentation realizes the hydrolysis and transformation of organic matter, the wastewater contains high concentrations of ammonia nitrogen, bicarbonate ions and soluble humic acid, which is very consistent with the raw material requirements for preparing conductive nano-calcium carbonate by the synchronous double decomposition coating method.
[0008] The black conductive nano-calcium carbonate prepared from biogas slurry has high specific surface area, excellent conductive properties, good thermal stability and chemical stability, and low cost. It becomes a conductive powder material. It can not only be used as a filler for polymer materials such as rubber and plastic, but also can solve the static electricity problem of polymer materials.
[0009] The technical solution adopted according to the present invention is as follows:
[0010] A method for preparing black conductive nano calcium carbonate by a biogas slurry synchronous double decomposition coating method comprises the following steps:
[0011] S1, separating the biogas slurry into solid and liquid, and collecting the separated liquid;
[0012] S2, determining the alkalinity molar concentration of the biogas slurry water separation liquid in step S1;
[0013] S3, according to the basicity molar concentration of the step calculated CaCl2 theoretical dosage, and according to the theoretical dosage of CaCl2, and the optimization coefficient k value further calculate the actual dosage of CaCl2;
[0014] S4, adding CaCl2 according to the actual dosage of CaCl2 to the biogas slurry water separation liquid in step S1, stirring until floccules are precipitated, and preparing a crude extract of humic acid-based nano calcium carbonate HA-CaCO3;
[0015] S5, centrifuging the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3, collecting the precipitate, drying, and carbonizing to obtain the black conductive nano-calcium carbonate; wherein, in step S5, the carbonization temperature is 400-650° C., and the carbonization time is 2-4 hours.
[0016] Step S2 is specifically as follows:
[0017] Determine the alkalinity molar concentration of the biogas slurry water separation liquid in step S1 according to equations (1) and (2);
[0018]
[0019]
[0020] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.
[0021] As another embodiment of the present invention, step S2 is specifically:
[0022] Dilute the biogas slurry separation liquid obtained in step S1 with distilled water, add methyl orange indicator, and according to formula (1), titrate the alkalinity of the biogas slurry separation liquid with HCl. Stop titration when the methyl orange indicator changes from orange-yellow to orange-red, and record the titration volume △V of acid H + ; Calculate the alkalinity of the biogas slurry according to equation (2);
[0023]
[0024]
[0025] Wherein: represents the molar concentration of the alkalinity of the biogas slurry, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample taken, L.
[0026] Step S3 is specifically as follows:
[0027] According to the molar concentration of the alkalinity of the biogas slurry in step S2, calculate the theoretical dosage of CaCl2 according to the metathesis reaction formula (3), and further calculate the actual dosage of CaCl2 according to the optimization coefficient k value;
[0028] CaCl2 + 2NH4HCO3 → CaCO3↓ + CO2↑ + 2NH4Cl + H2O (3)
[0029] 2HCl + CaCO3 → CaCl2 + H2O + CO2↑ (4)
[0030]
[0031]
[0032]
[0033] Wherein, represents the molar concentration of calcium chloride dosage, mol / L; k represents the dosage coefficient of calcium chloride. When k = 1, calcium chloride is the theoretical dosage molar concentration; when 0.5 < k < 1, calcium chloride is the actual dosage molar concentration; represents the molar mass concentration of calcium chloride, g / mol; N 沼液反应体积 represents the total volume of the biogas slurry reaction, L; represents the theoretical k = 1 or actual 0.5 < k < 1 dosage mass of calcium chloride, g.
[0034] Furthermore, step 3 includes the following steps:
[0035] According to the molar concentration of the alkalinity of the biogas slurry in step 2, according to the metathesis reaction formula (3) and formula (6), Ca 2+ / HCO3 - The molar ratio of the reaction is 1:2. The theoretically calculated dosage value of CaCl2 is 0.125 mol / L. According to the preset optimal value of the optimization coefficient k, which is 0.85, as shown in formula (6), it is 0.425 times the molar amount of alkalinity. The actual dosage of CaCl2 is 0.10625 mol / L. Because when Ca 2+ reacts with HCO3 - , the pH of the solution drops from 8.266 to 6.593. After the reaction, the biogas slurry is acidic, indicating that the concentration of free H + is higher than that of free OH - . Cl - combines with H + to form HCl, and reaction (4) will occur, causing the generated CaCO3 to decompose, resulting in free Ca 2+ . Also, due to the promotion of the hydrolysis of carbonic acid under acidic conditions, as shown in reaction formula (5), therefore, free Ca 2+ combines with HCO3 - to form a Ca(HCO3)2 solution, leading to excessive hardness. So, the actual dosage is 15% less than the theoretical dosage;
[0036] CaCl2 + 2NH4HCO3 → CaCO3↓ + CO2↑ + 2NH4Cl + H2O (3)
[0037] 2HCl + CaCO3 → CaCl2 + H2O + CO2↑ (4)
[0038]
[0039]
[0040]
[0041] Among them, represents the molar concentration of calcium chloride dosage, mol / L; k represents the dosage coefficient of calcium chloride. When k = 1, calcium chloride is the theoretically calculated molar concentration; when 0.5 < k < 1, calcium chloride is the actual molar concentration dosage (k = 0.85 is the preset optimal value); represents the molar mass concentration of calcium chloride, 111 g / mol; V 沼液反应体积 represents the reaction volume of the biogas slurry, L; represents the dosage mass of calcium chloride with theoretical k = 1 or actual 0.5 < k < 1, g.
[0042] The method for preparing black conductive nano-calcium carbonate by the biogas slurry synchronous double decomposition coating method also includes step S6: adding Ca(OH)2 emulsion to the supernatant after centrifugation of the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3 in step S5 under stirring, stirring for 10-20 minutes, and stopping the addition when the pH value is adjusted to 7.5-8; then adding NaOH solution to adjust the pH value to 8.3-8.5; continuing to stir until flocculent precipitates appear, collecting the precipitates, and obtaining the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3; centrifuging the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3, collecting the precipitates, drying, and carbonizing to obtain the black conductive nano-calcium carbonate.
[0043] The carbonization temperature is 400-650° C., and the carbonization time is 2-4 hours.
[0044] The Ca(OH)2 emulsion is prepared by mixing CaO and distilled water.
[0045] The black conductive nano calcium carbonate is prepared by the method for preparing black conductive nano calcium carbonate by the biogas slurry synchronous double decomposition coating method.
[0046] The present invention also seeks to protect the use of the above-mentioned black conductive nano calcium carbonate as a filler and antistatic agent in polymer insulating material products.
[0047] The polymer insulating material includes plastic and rubber.
[0048] Compared with the prior art, the advantages of the present invention are:
[0049] 1. The present invention adopts double decomposition coating method to prepare black conductive nano calcium carbonate in biogas slurry. That is, a soluble carbonate solution is added to a certain concentration of calcium chloride aqueous solution, and calcium carbonate precipitation is obtained after double decomposition reaction. Compared with the carbonization method, this method has the advantages of fast reaction rate and high efficiency. It belongs to liquid-liquid reaction, the reaction conditions are controllable, and it is easy to realize the study of reaction kinetics. Biogas slurry is rich in NH4 + 、HCO3 - , soluble humic acid organic matter, etc.; adding CaCl2 solution to the biogas slurry will cause a double decomposition reaction to form nano calcium carbonate crystal nuclei. Since the biogas slurry is rich in soluble humic acid organic matter, it will coat the surface of the crystal nucleus, inhibiting the unlimited growth of the crystal nucleus, which is beneficial to control the particle size of nano calcium carbonate and prevent agglomeration between particles. According to the double layer theory, the double layer of soluble humic acid organic matter still maintains electrical neutrality, but the number of positive ions decreases, that is, the thickness of the double layer becomes thinner, and the ξ potential on the sliding surface of the soluble humic acid organic matter is reduced to the critical potential ξ K , repulsive barrier E maxThe humic acid is destabilized and condensed; a large number of calcium carbonate microcrystals appear in the double decomposition reaction, and the Ca atoms in the surface molecules are easily chelated with the -OH and -COOH O atoms on the humic acid chain. The soluble humic acid in the biogas slurry is used to coat the calcium carbonate microcrystals, which has a strong molecular binding ability. The humic acid coating also prevents the agglomeration of the calcium carbonate crystals, overcoming the defects of the asynchronous coating method described in the background technology.
[0050] 2. This invention proposes for the first time to use soluble humic acid organic matter in biogas slurry to coat the nano calcium carbonate generated by double decomposition to prepare black conductive nano calcium carbonate, with a resistivity of 2.62×10 6 Ω·cm, reaching the resistivity of conductive powder (10 -5 ~10 9 Ω·cm) requirements;
[0051] 3. The biogas slurry is used to prepare black conductive nano-calcium carbonate through the synchronous double decomposition coating method, and the development of functional high-end products meets the market demand. It is of great significance to utilize the biogas slurry in a high-value way and realize the green and high-quality development of the natural gas industry;
[0052] 4. SEM observation showed that black nano-calcium carbonate was in the form of block aggregates; XRD characterization showed that it was a calcite crystal. XRF analysis showed that the C mass fraction was 5% higher than the actual C mass fraction of calcium carbonate, revealing the coating effect of biogas slurry carbon source on nano-calcium carbonate. TGA results revealed the reason why humic acid-based nano-calcium carbonate appeared black after carbonization at 550°C for 4 hours. At 700°C, it lost about 5% of its weight, which was consistent with the XRF analysis results. It was caused by the volatilization of the coated C in gaseous form. BET analysis showed that its specific surface area was 5.03m 2 ·g -1 , the total pore volume is 0.033 cm 3 ·g -1 The average pore size is 26.33nm, which is mesoporous. Raman spectroscopy shows that black nano calcium carbonate has a certain degree of order and is graphitized; the four-probe measurement shows that its resistivity is 2.62×10 6 Ω·cm, conductive, that is, conductive nano calcium carbonate, further developed into conductive powder, as a filler for plastics and rubber, it also has anti-static properties, eliminating the harm of static electricity;
[0053] 5. Design of strong electrolyte Cl for CaCl2 - Replacement of biogas slurry HCO3 - Experiment to solve the problem of weak electrolysis of HCO3 in biogas slurry - Effects on NH4 recovery by electrodialysis + , K + Low conductivity, high energy consumption and prevention of HCO3 caused by the process - With OH - The reaction produces CO3 2- , and biogas slurry Ca2+ The generation of CaCO3 precipitates causes membrane plugging problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0055] Figure 1 The diagram is a mechanism diagram of preparing conductive nano calcium carbonate by synchronous double decomposition and coating principle and method of biogas slurry and calcium chloride according to the present invention;
[0056] Figure 2 For: humic acid-based nano-calcium carbonate wet sample (HA-CaCO3) (a), humic acid-based nano-calcium carbonate dry sample (105℃ (12h) (b), black conductive nano-calcium carbonate (550℃ (4h) (c), black conductive nano-calcium carbonate in SEM 10 (000 magnification image (d) and 50 (000 magnification image (e);
[0057] Figure 3 For: XRD crystal phase diagram of black conductive nano calcium carbonate;
[0058] Figure 4 Thermogravimetric analysis and specific surface area analysis of black conductive nano calcium carbonate;
[0059] Figure 5 For: Raman analysis of black conductive nano calcium carbonate;
[0060] Figure 6 This is the principle diagram of the four-probe method for determining black conductive nano-calcium carbonate;
[0061] Figure 7 This is the product picture of black conductive nano calcium carbonate. DETAILED DESCRIPTION
[0062] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0063] The biogas slurry treated in the experimental process comes from the anaerobic fermentation tank effluent of Miaoji Biogas Station (32°38′7.68″N, 115°43′3.24″E) in Funan County, Fuyang City, Anhui Province, and the liquid separated by solid-liquid separation by the snail stacker. During the test period (April 1, 2022 to October 14, 2022), the COD of the biogas slurry was 4063-5207 mg / L, and the NH4 +-N is 2424~3024mg / L, containing HCO3 - The total alkalinity of ions (calculated as CaCO3) is 8759~14264 mg / L, the hardness (calculated as CaCO3) is 70~220 mg / L, the pH is 8.113~8.327, and the water temperature is 14.1~29.4℃.
[0064] The reagents required for the test process: calcium chloride, calcium oxide, sodium hydroxide, pure sodium carbonate, hydrogen peroxide, anhydrous ethanol, hydrochloric acid, all of which are AR grade.
[0065] Synchronous metathesis coating theory, mixing organic polymers with inorganic precursors in a solvent, so that the inorganic precursors chemically synthesize nanoparticles and fill them into polymer aggregates at the same time. The presence of polymers can effectively control the particle size growth of inorganic nanoparticles and prevent the agglomeration of nanoparticles; the mechanism of preparing black conductive nano-calcium carbonate from biogas slurry, see Figure 1 .
[0066] Example 1 Preparation of black conductive nano calcium carbonate
[0067] This embodiment provides a method for preparing black conductive nano calcium carbonate from biogas slurry, comprising the following steps:
[0068] Step 1, specifically taking the biogas slurry water from the anaerobic fermentation tank of Miaoji Biogas Station in Funan County, Anhui Province as an example, the biogas slurry water from the anaerobic fermentation tank first passes through a screw stacker for solid-liquid separation, and the biogas slurry separation liquid is collected.
[0069] Step 2: Take 1 mL of the biogas slurry separation solution (V) from step 1 above and put it into a 250 mL clean conical flask, dilute it 50 times with distilled water, add 4 drops of methyl orange indicator, and according to the reaction principle, see formula (1), titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl. When the methyl orange indicator changes from orange to red, stop the titration and record the hydrochloric acid (H + )’s titration volume △V = 5.00 mL; According to equation (2), the alkalinity of the biogas slurry is calculated to be 0.25 mol / L.
[0070]
[0071]
[0072] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.
[0073] Step 3, take 1 mL of the biogas slurry separated liquid after the solid-liquid separation in the above step 1 into a colorimetric tube, dilute it to 10 mL with distilled water, and use the "Technical Requirements and Detection Methods for COD Photometric Rapid Determination Instrument" (HJ 924-2017) and a multi-parameter water quality analyzer (5B-3B (V8) (Lianhua Technology Company) to perform spectrophotometric determination of the soluble humic acid organic matter in the biogas slurry, which is 4018 mg / L (in terms of chemical oxygen demand (COD)).
[0074] Step 4: Based on the molar concentration of alkalinity of the biogas slurry in step 2, according to the double decomposition reaction formula (3) and formula (6), Ca 2+ / HCO3 - The molar ratio of CaCl2 is 1:2, and the calculated theoretical dosage of CaCl2 is 0.125 mol / L. According to formula (6), the optimal value of 0.85 is preset according to the optimization coefficient k, which is 0.425 times the molar amount of alkalinity. The actual dosage of CaCl2 is 0.10625 mol / L. 2+ With HCO3 - After the reaction, the pH of the solution decreased from 8.266 to 6.593. The biogas slurry was acidic after the reaction, indicating that the free H + The concentration is higher than free OH - High concentration, Cl - With H + HCl is formed, and an acidification reaction occurs, see reaction formula (4), which decomposes the generated CaCO3 and produces free Ca 2+ Since the hydrolysis of carbonic acid is promoted under acidic conditions, see reaction (5), free Ca 2+ With HCO3 - Combined, forming Ca(HCO3)2 solution, resulting in excessive hardness. Therefore, the actual dosage is 15% smaller than the theoretical dosage.
[0075] CaCl2+2NH4HCO3→CaCO3↓+CO2↑+2NH4Cl+H2O (3)
[0076] 2HCl+CaCO3→CaCl2+H2O+CO2↑ (4)
[0077]
[0078]
[0079]
[0080] in, It represents the molar concentration of calcium chloride added, mol / L; k represents the addition coefficient of calcium chloride. When k=1, the calcium chloride is the theoretical addition molar concentration; when k=0.85, the calcium chloride is the actual addition molar concentration; represents the molar mass concentration of calcium chloride, 111 g / mol; V 沼液反应体积 represents the total volume of biogas slurry reaction, L; Indicates the theoretical or actual added mass of calcium chloride, g.
[0081] Step 5, according to steps 3 and 4, take 1L of the biogas slurry separation liquid of step 1 and pour it into a clean beaker, and place it on a magnetic stirrer and stir it at a speed of 500r / min; according to formulas (6) and (7), the actual CaCl2 molar dosage is 0.10625mol / L, and the added mass of CaCl2 (AR) is calculated to be 11.79g, which is dissolved in 17mL of distilled water; the CaCl2 solution is slowly added to the beaker with a glass rod, and the timing starts when the CaCl2 liquid is added, and the magnetic stirring is performed for 10min, and the mixture is allowed to stand for 20min. During the stirring process, a flocculent substance precipitates, and after standing, the floating substance is accompanied by the generation of continuous small bubbles. According to the double decomposition reaction formula (3) and the synchronous double decomposition coating theory, when the CaCO3 precipitation is generated, the biogas soluble humic acid coats the CaCO3 crystal nucleus to form a humic acid-based nano calcium carbonate (HA-CaCO3) crude extract, and record sample 1.
[0082] Step 6, centrifuge the HA-CaCO3 crude extract sample of step 5 to separate the solid and liquid, collect the precipitate and put it into an oven to dry at 105° C. for 10 hours, cool it, and obtain a HA-CaCO3 dry sample.
[0083] Step 7, pour the HA-CaCO3 dried sample of step 6 into a round-bottom crucible, cover the crucible with a lid, wrap it with tin foil, put it into a muffle furnace and carbonize it at 550°C for 4 hours, and cool it to obtain black conductive nano-calcium carbonate (sample 1 final product).
[0084] Example 2 Preparation of black conductive nano calcium carbonate
[0085] This embodiment provides a method for preparing black conductive nano calcium carbonate from biogas slurry, comprising the following steps:
[0086] Step 1, specifically taking the biogas slurry water from the anaerobic fermentation tank of Miaoji Biogas Station in Funan County, Anhui Province as an example, the biogas slurry water from the anaerobic fermentation tank first passes through a screw stacker for solid-liquid separation.
[0087] Step 2: Take the separated liquid biogas slurry V = 1 mL from step 1 above and put it into a 250 mL clean conical flask, dilute it 50 times with distilled water, add 4 drops of methyl orange indicator, and according to the reaction principle, see formula (1), use 0.05 mol / L HCl to titrate the alkalinity of the biogas slurry. When the methyl orange indicator changes from orange to orange, stop the titration and record the hydrochloric acid (H + )’s titration volume △V = 5.00 mL; According to formula (2), the alkalinity of the biogas slurry is calculated to be 0.25 mol / L.
[0088]
[0089]
[0090] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.
[0091] Step 3, take the biogas slurry separated liquid after the solid-liquid separation in the above step 1, take 1 mL of the biogas slurry into a colorimetric tube, dilute it to 10 mL with distilled water, and use the "Technical Requirements and Detection Methods for COD Photometric Rapid Determination Instrument" (HJ 924-2017) and a multi-parameter water quality analyzer (5B-3B (V8), Lianhua Technology Co., Ltd.) to perform spectrophotometric determination of the soluble humic acid organic matter in the biogas slurry, which is 4018 mg / L (in terms of chemical oxygen demand (COD)).
[0092] Step 4: Based on the molar concentration of alkalinity of the biogas slurry in step 2, according to the double decomposition reaction formula (3) and formula (6), Ca 2+ / HCO3 - The molar ratio of CaCl2 is 1:2, and the calculated theoretical dosage of CaCl2 is 0.125 mol / L. According to formula (6), according to the preset optimal value of the optimization coefficient k of 0.85, that is, 0.425 times the molar amount of alkalinity is added, and the actual dosage of CaCl2 is 0.10625 mol / L. 2+ With HCO3 - After the reaction, the pH of the solution decreased from 8.266 to 6.593. The biogas slurry was acidic after the reaction, indicating that the free H + The concentration is higher than free OH - High concentration, Cl - With H + When HCl is formed, reaction (4) will occur, causing the generated CaCO3 to decompose and free Ca 2+ Since the hydrolysis of carbonic acid is promoted under acidic conditions, see reaction (5), free Ca 2 +With HCO3 - Combined, forming Ca(HCO3)2 solution, resulting in excessive hardness. Therefore, the actual dosage is 15% smaller than the theoretical dosage.
[0093] CaCl2+2NH4HCO3→CaCO3↓+CO2↑+2NH4Cl+H2O (3)
[0094] 2HCl+CaCO3→CaCl2+H2O+CO2↑ (4)
[0095]
[0096]
[0097]
[0098] in, It represents the molar concentration of calcium chloride added, mol / L; k represents the addition coefficient of calcium chloride. When k=1, the calcium chloride is the theoretical addition molar concentration; when k=0.85, the calcium chloride is the actual addition molar concentration; represents the molar mass concentration of calcium chloride, 111 g / mol; V 沼液反应体积 represents the biogas slurry reaction volume, L; Indicates the theoretical or actual added mass of calcium chloride, g.
[0099] Step 5, according to steps 3 and 4, take 1L of the biogas slurry separation liquid of step 1 and pour it into a clean beaker, and place it on a magnetic stirrer and stir it at a speed of 500r / min; according to formulas (6) and (7), the actual CaCl2 molar dosage is 0.10625mol / L, and the added mass of CaCl2 (AR) is calculated to be 11.79g, which is dissolved in 17mL of distilled water; the CaCl2 solution is slowly added to the beaker with a glass rod, and the timing starts when the CaCl2 liquid is added, and the magnetic stirring is performed for 10min, and the mixture is allowed to stand for 20min. During the stirring process, a flocculent substance precipitates, and after standing, the floating substance is accompanied by the generation of continuous small bubbles. According to the double decomposition reaction formula (3) and the synchronous double decomposition coating theory, when the CaCO3 precipitation is generated, the biogas soluble humic acid coats the CaCO3 crystal nucleus to form a humic acid-based nano calcium carbonate (HA-CaCO3) crude extract, and record sample 1.
[0100] Step 6, centrifuge the crude extract of HA-CaCO3 sample 1 in step 5 to separate the solid and liquid, collect the precipitate and put it into an oven at 105°C for 10 hours, cool it, and obtain a HA-CaCO3 dry sample.
[0101] Step 7, pour the HA-CaCO3 dried sample of step 6 into a round-bottom crucible, cover the crucible with a lid, wrap it with tin foil, put it into a muffle furnace and carbonize it at 550°C for 4 hours, and cool it to obtain black conductive nano-calcium carbonate (sample 1 final product).
[0102] Step 8, collect the centrifugal liquid of the HA-CaCO3 sample 1 centrifuged in step 6 into a dry beaker, continue to stir on a magnetic stirrer, and rotate at 500r / min; prepare Ca(OH)2 emulsion with CaO(AR) and distilled water, and slowly add it into the beaker by glass rod drainage until the pH value of the beaker solution rises from 6.593 to 7.900, stop adding, start recording the continuous stirring time for 10min, and keep the pH stable, adjust the pH to 8.300 with 1mol / L NaOH(AR) solution, stop adding, start recording the continuous stirring time for 10min, and keep the pH stable, and let it stand for 20min. Similar to the result of step 5, flocculation precipitation occurs, and no floating objects or small bubbles are generated. The generated flocculent precipitate is humic acid-based nano calcium carbonate (HA-CaCO3) according to reaction formulas (8) and (9) and the theory and method of synchronous double decomposition coating, and record sample 2.
[0103] Ca(OH)2+Ca(HCO3)2→2CaCO3↓+2H2o (8)
[0104] 2NaOH+Ca(HCO3)2→CaCO3↓+Na2CO3+2H2O (9)
[0105] Step 9, centrifuge the HA-CaCO3 sample 2 of step 8 to separate the solid and liquid, collect the solid sample and put it into an oven at 105° C. to dry for 10 hours, cool it, and obtain a HA-CaCO3 dry sample.
[0106] Step 10, pour the HA-CaCO3 dried sample of step 9 into a round-bottom crucible, cover the crucible with a lid, wrap it with tin foil, put it into a muffle furnace and carbonize it at 550°C for 4 hours, and cool it to obtain black conductive nano-calcium carbonate (sample 2 final product).
[0107] Example 3 Preparation of Conductive Nano-Calcium Carbonate
[0108] This embodiment provides a method for preparing black conductive nano calcium carbonate from biogas slurry, comprising the following steps:
[0109] Step 1, specifically taking the biogas slurry water from the anaerobic fermentation tank of Miaoji Biogas Station in Funan County, Anhui Province as an example, the biogas slurry water from the anaerobic fermentation tank first passes through a screw stacker for solid-liquid separation.
[0110] Step 2: Take 1 mL of the biogas slurry V of the separation liquid in step 1 above and put it into a 250 mL clean conical flask, dilute it 50 times with distilled water, add 4 drops of methyl orange indicator, and according to the reaction principle, see formula (1), titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl. When the methyl orange indicator changes from orange to orange, stop the titration and record the hydrochloric acid (H + )’s titration volume △V = 5.00 mL; According to equation (2), the alkalinity of the biogas slurry is calculated to be 0.25 mol / L.
[0111]
[0112]
[0113] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.
[0114] Step 3, take the biogas slurry separated liquid after the solid-liquid separation in the above step 1, take 1 mL of the biogas slurry into a colorimetric tube, dilute it to 10 mL with distilled water, and use the "Technical Requirements and Detection Methods for COD Photometric Rapid Determination Instrument" (HJ 924-2017) and a multi-parameter water quality analyzer (5B-3B (V8) (Lianhua Technology Company) to perform spectrophotometric determination of the soluble humic acid organic matter of the biogas slurry, which is 4018 mg / L (in terms of chemical oxygen demand (COD)).
[0115] Step 4: Based on the molar concentration of alkalinity of the biogas slurry in step 2, according to the double decomposition reaction formula (3) and formula (6), Ca 2+ / HCO3 - The molar ratio of CaCl2 is 1:2, and the calculated theoretical dosage of CaCl2 is 0.125 mol / L. According to formula (6), the actual dosage is 0.10625 mol / L according to the preset optimal value of the dosage coefficient k of 0.85, which is 0.425 times the molar amount of alkalinity. 2+ With HCO3 - After the reaction, the pH of the solution decreased from 8.266 to 6.593. The biogas slurry was acidic after the reaction, indicating that the free H + The concentration is higher than free OH - High concentration, Cl - With H + The formation of HCl will cause an acidification reaction, which will decompose the generated CaCO3 and produce free Ca 2+ , see reaction (4). Also, under acidic conditions, the hydrolysis of carbonic acid is promoted, see reaction (5), so free Ca 2+ With HCO3- Combined, forming Ca(HCO3)2 solution, resulting in excessive hardness. Therefore, the actual dosage is 15% smaller than the theoretical dosage.
[0116] CaCl2+2NH4HCO3→CaCO3↓+CO2↑+2NH4Cl+H2O (3)
[0117] 2HCl+CaCO3→CaCl2+H2O+CO2↑ (4)
[0118]
[0119]
[0120]
[0121] in, It represents the molar concentration of calcium chloride added, mol / L; k represents the addition coefficient of calcium chloride. When k=1, the calcium chloride is the theoretical addition molar concentration; when k=0.85, the calcium chloride is the actual addition molar concentration; represents the molar mass concentration of calcium chloride, 111 g / mol; V 沼液反应体积 Represents the total volume of biogas slurry reaction, L; Indicates the theoretical or actual added mass of calcium chloride, g.
[0122] Step 5, according to steps 3 and 4, 4t of sludge from the sludge was taken into the reaction barrel, and the pilot-scale agitator was turned on; according to formulas (6) and (7), the actual CaCl2 molar dosage was 0.10625mol / L, and the mass of CaCl2 (industrial grade, 74%) was calculated to be 63.75kg, which was added to the reaction barrel by a dry feeder until it was added, and the timing was started. After magnetic stirring for 10 minutes, the solution entered the vertical flow sedimentation tank and was allowed to settle. During the stirring process, a flocculated substance appeared, and the flocculated substance was allowed to settle. According to the double decomposition reaction formula (3) and the synchronous double decomposition coating theory, when the CaCO3 precipitate was generated, the sludge soluble humic acid coated the CaCO3 crystal nucleus to form humic acid-based nano calcium carbonate (HA-CaCO3), and sample 1 was recorded.
[0123] Step 6, take the HA-CaCO3 sample 1 of step 5 and centrifuge it to separate the solid and liquid, take a small part of the solid after solid-liquid separation, put it into an oven at 105°C and dry it for 10 hours, cool it, and obtain a HA-CaCO3 dry sample.
[0124] Step 7, pour the HA-CaCO3 dried sample of step 6 into a round-bottom crucible, cover the crucible with a lid, wrap it with tin foil, put it into a muffle furnace and carbonize it at 550°C for 4 hours, and cool it to obtain black conductive nano-calcium carbonate (sample 1 final product).
[0125] Step 8, according to step 5, the static supernatant enters the next 4t reaction barrel, and the pilot mixer is turned on, and CaO (industrial grade, 84%) is slowly added to the reaction barrel by a feeder. According to reaction formula (8), the pH in the reaction barrel reaches 7.9; according to reaction formula (9), 1mol / L NaOH solution is continued to be added to the reaction barrel to react until pH=8.3 and then the addition is stopped. Stirring is continued for 10min, and the reaction liquid is allowed to stand for 20min in the next vertical flow sedimentation tank. During the stirring process, a flocculated substance appears, and the flocculated substance is allowed to stand and settle. According to reaction formulas (8) and (9) and the theory and method of synchronous double decomposition coating, the generated flocculated precipitate is humic acid-based nano calcium carbonate (HA-CaCO3), and sample 2 is recorded.
[0126] Ca(OH)2+Ca(HCO3)2→2CaCO3↓+2H2O (8)
[0127] 2NaOH+Ca(HCO3)2→CaCO3↓+Na2CO3+2H2O (9)
[0128] Step 9, centrifuge the HA-CaCO3 sample 2 of step 8 to separate the solid from the liquid, take a small portion of the solid after the solid-liquid separation, put it into an oven at 105° C. and dry it for 10 hours, and cool it.
[0129] Step 10, pour the HA-CaCO3 dried sample of step 9 into a round-bottom crucible, cover the crucible with a lid, wrap it with tin foil, put it into a muffle furnace and carbonize it at 550°C for 4 hours, and cool it to obtain black conductive nano-calcium carbonate (sample 2 final product).
[0130] Comparative Example 1
[0131] The difference between this comparative example and Example 1 is that the (CaCl2) substance is replaced by HCl to react with HCO3 in the biogas slurry. - Reaction, see equation (10), although the weak electrolyte HCO3 in the biogas slurry is solved - The problem is that it will lead to CO2 emissions, causing environmental problems, and will not produce humic acid-based nano-calcium carbonate, and it is impossible to obtain black conductive nano-calcium carbonate.
[0132]
[0133] Comparative Example 2
[0134] The difference between this comparative example and Example 1 is that the (CaCl2) substance is replaced by H2SO4, which reacts with HCO3 in the biogas slurry. - Reaction, see equation (10), although the weak electrolyte HCO3 in the biogas slurry is solved -The problem is that it will lead to CO2 emissions, causing environmental problems, and will not produce humic acid-based nano-calcium carbonate, and it is impossible to obtain black conductive nano-calcium carbonate.
[0135]
[0136] Comparative Example 3
[0137] The difference between this comparative example and Example 1 is that no (CaCl2) substance is added, and the HCO3 in the biogas slurry - The solution exists in a free state, no humic acid-based nano-calcium carbonate is produced, and black conductive nano-calcium carbonate cannot be obtained.
[0138] Comparative Example 4
[0139] The difference between this comparative example and Example 1 is that the biogas slurry is replaced by biomass rice bran, which is a coated solid. According to reaction equations (3) to (7), a wet sample of nano-calcium carbonate without humic acid coating is first obtained, which is further dried. The dried nano-calcium carbonate is used as a template and mixed with biomass in a certain proportion to obtain black nano-calcium carbonate. This method belongs to a multi-step method for preparing black nano-calcium carbonate, and its effect is not as strong as the black nano-calcium carbonate obtained by the simultaneous double decomposition and coating reaction of soluble humic acid in the biogas slurry.
[0140] Performance test case
[0141] 1. Characterization methods
[0142] The morphology of black nano-calcium carbonate prepared from biogas slurry was analyzed by SEM (ZEISS GeminiSEM 300, Germany); the phase and elemental composition of black nano-calcium carbonate were analyzed by X-ray diffractometer (XRD, Rigaku Ultima IV, Japan) and X-ray fluorescence spectrometer (XRF (SHIMADZU XRF-1800, Japan); the mass change of black nano-calcium carbonate at different temperatures was analyzed by thermogravimetric analyzer (TG (Mettler STAR, Switzerland); the specific surface area, total pore volume and pore size of black nano-calcium carbonate and carbon-based materials were determined and analyzed by BET instrument (BELSORP MR1, MicrotracBEL, Japan); the structural characteristics and properties of black nano-calcium carbonate were characterized by Raman spectrometer (Raman, Hori (a La (RAM HR Evolution, Japan); and the conductivity of black nano-calcium carbonate powder was determined by four-probe instrument (RTS-2, Guangzhou Four Probe Co., Ltd.).
[0143] 2. Results
[0144] 2.1 Product morphology characteristics
[0145] Figure 2 The morphology of black conductive nano-calcium carbonate (HA-CaCO3) generated by the double decomposition reaction of biogas slurry and CaCl2 to coat soluble humic acid organic matter and then carbonized at 550℃ for 4h is shown. Figure 2 (a) is the wet sample of humic acid-based nano-calcium carbonate (HA-CaCO3) generated by the reaction of biogas slurry and CaCl2. Figure 2 (b) is the sample of humic acid-based nano-calcium carbonate (HA-CaCO3) after being dried at 105℃ for 12h. Figure 2 (c) is a black conductive nano-calcium carbonate sample formed by humic acid-based nano-calcium carbonate (HA-CaCO3) after oxygen-free carbonization at 550℃ for 4h. The black conductive nano-calcium carbonate is observed under a 10000x microscope in the form of a wrapped sheet ( Figure 2 d), observed under a 50,000x microscope, the aggregates are irregular, unevenly sized cubes, belonging to the calcite type ( Figure 2 e). The black conductive nanoparticles are relatively large in size and have obvious agglomeration ( Figure 2 d, e), which is related to the high surface activation energy of calcium carbonate and the carbon skeleton connection formed by humic acid after high temperature carbonization.
[0146] 2.2 Crystal structure and composition
[0147] Figure 3 It is the XRD diffraction peak of black conductive nano calcium carbonate. Calcium carbonate has diffraction peaks at 2θ=23.0, 29.4, 36.0, 39.4, 43.1, 47.5, 48.5, 56.4, and 57.5°, corresponding to (012), (104), (110), (113), (202), (018), (116), (211), and (122) crystal planes, respectively, indicating that the crystal form of calcium carbonate is calcite. Calcite calcium carbonate is thermodynamically the most stable than aragonite and vaterite calcium carbonate. The XRF elemental composition analysis of black conductive nano calcium carbonate classifies the elemental composition with a proportion greater than 10%, as shown in Table 1. The results show that the main elemental components of black conductive nano calcium carbonate are Ca, O, and C, which just further proves the analysis results of XRD. The mass fractions of Ca, O and C in anhydrous calcium carbonate are 40%, 48% and 12% respectively. The C component in XRF analysis is 5% higher than the actual calcium carbonate component, revealing that this part of carbon comes from the coating effect of soluble humic acid organic matter in the biogas slurry.
[0148] Table 1 XRF composition analysis of black conductive nano calcium carbonate
[0149]
[0150] 2.3 Thermogravimetry and specific surface area
[0151] Figure 4 (a) is the TG curve of black conductive nano-calcium carbonate. When the temperature rises to about 630°C, the weight loss of black conductive nano-calcium carbonate is about 2.5% (point 1), which is related to the volatilization of bound water and part of the carbon, explaining why humic acid-based nano-calcium carbonate (HA-CaCO3) is still black after carbonization at 550°C for 4 hours. When the temperature rises to 800°C, the weight loss of black conductive nano-calcium carbonate is about 42.5% (point 2), indicating that black conductive nano-calcium carbonate is completely decomposed at this high temperature. At 700°C, its weight loss is about 5%, which is a coated carbon material and has not decomposed itself. Figure 4 (( and c) are the N2 adsorption-desorption isotherms of black conductive nano-calcium carbonate. With the increase of relative pressure, the adsorption amount increases in a curve. When the relative pressure P / P0>0.4, the isotherm has a hysteresis loop, indicating that the black conductive nano-calcium carbonate has mesoporous properties. The BET specific surface areas of black conductive nano-calcium carbonate are 5.03m 2 ·g -1 , the total pore volume is 0.033 cm 3 ·g -1 , the average pore size is 26.33nm.
[0152] 2.4 Graphitization and conductivity
[0153] Figure 5 This is the Raman spectrum of black conductive nano-calcium carbonate. -1 and 1590cm -1 There are two characteristic peaks, which are respectively attributed to the defect vibration of the carbon atom lattice (D peak) and the stretching vibration of the sp2 carbon atom (G peak). The intensity ratio of D peak to G peak is D / I G Represents the degree of graphitization of carbon materials, I D / I G The lower the value, the higher the order and integrity of the carbon. The results of this study show that black conductive nano-calcium carbonate has a certain degree of order and graphitization exists. The resistivity and conductivity results of black conductive nano-calcium carbonate and the comparative values of the resistivity and conductivity of other materials are shown in Table 2. The resistivity and conductivity of black conductive nano-calcium carbonate are 2.62×10 6 Ω·cm and 3.8×10 -7 S cm -1 The resistivity of black conductive nano calcium carbonate is lower than that of calcium carbonate and silica coated calcium carbonate, indicating better conductivity. The resistivity of black conductive nano calcium carbonate is within the required resistivity of conductive powder (10 -5 ~10 9 Ω·cm) range, and has the potential to develop conductive powders.
[0154] Table 2 Comparison of resistivity and conductivity of black conductive nano calcium carbonate, CaCO3 and CaCO3-SiO2 materials
[0155]
[0156] SEM test method: Take a trace amount of black conductive nano-calcium carbonate sample and stick it directly to the conductive glue, and use QuorumSC7620 sputtering coater to spray gold for 45s (the specific spraying time is determined according to the sample / test requirements), and the gold spraying current is 10mA; then use ZEISS GeminiSEM 300 scanning electron microscope to take pictures of sample morphology, energy spectrum mapping and other tests. The acceleration voltage is 3kV when taking morphology, and the acceleration voltage is 15kV when taking energy spectrum mapping. The detector is SE2 secondary electron detector.
[0157] XRD test method: X-ray diffraction analysis of the sample was carried out on an X-ray diffractometer (Rigaku Ultima IV), with CuKα as the radiation source wavelength of 0.15418nm, the test range of 10° to 90°, the scanning speed of 0.02° / s, the tube voltage of 40kV and the current of 40mA.
[0158] TG test method: Using a thermogravimetric analyzer (Mettler STAR), in a static N2 atmosphere, in the range of 20-1000°C, with a heating rate of 10°C / min, the carbonization, decomposition, and weight loss of black conductive nano-calcium carbonate with temperature were measured.
[0159] XRF test method: On the X-ray fluorescence spectrometer (SHIMADZU XRF-1800), first turn on the external cooling water, then turn on the instrument power, the "RUN" indicator on the host panel is on, turn on the PC power, start the Windows operating system, start the PC-XRF software, click Analysis, click Sample Registration, select Analysis, and perform quantitative analysis of the elemental composition of the black conductive nano calcium carbonate powder sample.
[0160] Raman spectroscopy test method: Raman spectrometer (Raman (Japan Hori (a La (RAM HR Evolution)) is used, the Raman spectrum laser wavelength is 514nm, and the scanning range is 500~3000cm -1 .
[0161] BET test method: Using a BET instrument (BELSORP MR1), the specific surface area and pore size distribution curve of porous materials are determined by nitrogen low-temperature adsorption method. The sample is heated and vacuumed to remove impurity gases adsorbed on the surface. Then it is weighed and placed in liquid nitrogen. At liquid nitrogen temperature, the nitrogen adsorption of the sample is measured at different pre-set pressure points to obtain the adsorption isotherm. Then the data is processed by computer to calculate the specific surface area, pore volume, average pore size and pore size distribution from the adsorption isotherm.
[0162] Four-probe instrument test method: Four probes (RTS-2) arranged in a straight line are pressed vertically on the surface of the black conductive nano-calcium carbonate sample to be tested with a certain pressure. A current of 1 (mA) is passed between probes 1 and 4, and a certain voltage V (mV) is generated between probes 2 and 3. Figure 6 This voltage is measured and calculated according to the following formula (11) depending on the measurement method and sample size.
[0163]
[0164] Where D is the diameter of the black conductive nano-calcium carbonate sample, in cm or mm. Please note that it should be consistent with the probe spacing S.
[0165] S——average probe spacing, unit: cm or mm, please note that it should be consistent with the unit of sample diameter D (S value on the four-probe head certificate);
[0166] W——the thickness of the black conductive nano-calcium carbonate sample, unit: cm, please note that it should be consistent with the unit of S in F(W / S);
[0167] Fsp——Probe spacing correction factor (F value on the four-probe head certificate);
[0168] F(D / S)——sample diameter correction factor. When D→∞, F(D / S)=4.532, and the F(D / S) under finite diameter can be found in Appendix B;
[0169] F(W / S)——sample thickness correction factor. When W / S<0.4, F(W / S)=1; when W / S>0.4, the F(W / S) value can be found in Appendix C;
[0170] I——The current value flowing through probes 1 and 4. Please refer to Table 3 for the selected value.
[0171] V——The voltage value taken between probes 2 and 3, in mV.
[0172] Table 3 Current range selection for resistivity measurement
[0173] Resistivity (Ω·cm) Current range <0.03 100mA 0.03~0.3 10mA 0.3~30 1mA 30~300 100μA 300~3000 10μA >3000 1μA
[0174] Table 4 Characterization parameters
[0175]
[0176] 3D Structure:
[0177] Black conductive nano-calcium carbonate: carbon-coated cube-shaped morphology, calcite crystal type
[0178] Electrical conductivity:
[0179] Black conductive nano calcium carbonate: graphitized, resistivity 2.62×10 6 Ω·cm, has electrical conductivity.
[0180] Samples of black conductive nano calcium carbonate, see Figure 7 .
[0181] In the description of the present application, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0182] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A method for preparing black conductive nano-calcium carbonate by synchronous double decomposition and coating of biogas slurry, characterized in that: The following steps are involved: S1, separating the biogas slurry into solid and liquid, and collecting the separated liquid; S2, determining the alkalinity molar concentration of the biogas slurry water separation liquid in step S1; S3, according to the alkalinity molar concentration of step S2, the theoretical dosage of CaCl2 is calculated, and the actual dosage of CaCl2 is calculated according to the optimization coefficient k value of the theoretical dosage of CaCl2; S4, adding CaCl2 according to the actual dosage of CaCl2 to the biogas slurry water separation liquid in step S1, stirring until floccules are precipitated, and preparing a crude extract of humic acid-based nano calcium carbonate HA-CaCO3; S5, centrifuging the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3, collecting the precipitate, drying, and carbonizing to obtain the black conductive nano-calcium carbonate; wherein the carbonization temperature is 400-650° C., and the carbonization time is 2-4 hours; Step S2 is specifically as follows: Determine the alkalinity molar concentration of the biogas slurry water separation liquid in step S1 according to equations (1) and (2); in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; C H+ represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L; Step S3 is specifically as follows: According to the molar concentration of alkalinity of the biogas slurry in step S2, the theoretical dosage of CaCl2 is calculated according to the double decomposition reaction formula (3), and the actual dosage of CaCl2 is further calculated according to the optimization coefficient k; CaCl2+2NH4HCO3→CaCO3↓+CO2↑+2NH4Cl+H2O (3) 2HCl+CaCO3→CaCl2+H2O+CO2↑ (4) Among them, represents the molar concentration of calcium chloride addition, mol / L; k represents the addition coefficient of calcium chloride. When k = 1, calcium chloride is the theoretical molar concentration addition amount; when 0.5 < k < 1, calcium chloride is the actual molar concentration addition amount. represents the molar mass concentration of calcium chloride, g / mol; V biogas slurry reaction volume represents the volume of biogas slurry in the reaction, L. represents the theoretical k = 1 or actual 0.5 < k < 1 addition mass of calcium chloride, g.
2. The method for preparing black conductive nano-calcium carbonate by synchronous metathesis coating of biogas slurry according to claim 1, characterized in that: Step S2 is specifically as follows: Take the biogas slurry separation liquid from step S1 and dilute it with distilled water, add methyl orange indicator, and titrate the alkalinity of the biogas slurry separation liquid with HCl according to formula (1). When the methyl orange indicator changes from orange to red, stop the titration and record the acid H + The titration volume △V; According to equation (2), the alkalinity of the biogas slurry is calculated; in: Indicates the molar concentration of alkalinity of biogas slurry, mol / L; C H+ It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.
3. The method for preparing black conductive nano-calcium carbonate by synchronous metathesis coating of biogas slurry according to claim 1, characterized in that: The method also includes step S6: adding Ca(OH)2 emulsion to the supernatant after centrifugation of the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3 in step S5 under stirring, stirring for 10-20 minutes, and stopping the addition when the pH value is adjusted to 7.5-8; then adding NaOH solution to adjust the pH value to 8.3-8.5; continuing stirring until flocculent precipitates appear, collecting the precipitates, and obtaining the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3; centrifuging the crude extract of humic acid-based nano-calcium carbonate HA-CaCO3, collecting the precipitates, drying, and carbonizing to obtain the black conductive nano-calcium carbonate.
4. The method for preparing black conductive nano-calcium carbonate by synchronous metathesis coating of biogas slurry according to claim 3, characterized in that: The carbonization temperature is 400-650° C., and the carbonization time is 2-4 hours.
5. The method for preparing black conductive nano-calcium carbonate by synchronous metathesis coating of biogas slurry according to claim 3, characterized in that: The Ca(OH)2 emulsion is prepared by mixing CaO and distilled water.
6. A black conductive nano-calcium carbonate prepared by the method for preparing black conductive nano-calcium carbonate by the biogas slurry synchronous double decomposition coating method as claimed in any one of claims 1 to 5.
7. Use of the black conductive nano calcium carbonate as claimed in claim 6 as a filler and antistatic agent in polymer insulating material products.
8. The use according to claim 7, characterized in that: The polymer insulating material includes plastic and rubber.