A method for resource utilization of titanium gypsum
By mixing ferrous ferrous ferrous ferrous gypsum with titanium gypsum and adding fluorine-containing wastewater and phosphate precipitant to control the pH value, the efficient removal of iron in titanium gypsum and calcium precipitation is achieved, the treatment problems of titanium gypsum and ferrous gypsum are solved, and resource recycling is improved Utilization and process simplicity reduce costs.
Patent Information
- Application Number
- CN202310499802.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-06
AI Technical Summary
The by-products such as titanium gypsum and ferrous yellow in the production process of titanium dioxide produced during the sulfuric acid titanium dioxide contain trivalent iron impurities, which makes them light red in color and cannot be directly used to prepare building materials gypsum boards. The comprehensive utilization rate is low, the processing is complex and the cost is high. Causes waste of land resources and environmental hazards.
Mix ferrous sulfate in the titanium dioxide process with titanium gypsum, add fluorine-containing wastewater and phosphate precipitant to control pH value, and form high-purity ferrous sulfate heptahydrate or polymeric sulfuric acid through solid-liquid separation and flocculation process. Iron removes calcium and iron impurities and improves the quality of titanium gypsum.
The removal of 90% of iron in titanium gypsum has been achieved, the quality of titanium gypsum has been improved, the stacking problems of titanium gypsum and ferrous yellow has been solved, the processing difficulty and cost has been reduced, the resource recycling rate has been improved, and the process flow has been simplified.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium dioxide preparation, and specifically relates to a method for resource utilization of titanium gypsum. Background Art
[0002] A large amount of acidic wastewater is generated during the production of titanium dioxide by sulfuric acid. Acidic wastewater mainly comes from titanic acid washing, acidolysis, calcination waste gas cooling washing wastewater, etc. Lime (or carbide slag) is usually added to neutralize the acidic wastewater to produce industrial sludge with CaSO4·2H2O as the main component, that is, titanium gypsum neutralization slurry, which belongs to general solid waste, with free water of about 40% to 60%, neutral pH value, and the main impurities on wet basis are Fe(OH)3 and Al2(SO4)3, and the Fe content is about 8%-14%. Titanium gypsum is light red in color due to the presence of trivalent iron impurities, and cannot be directly used to prepare building material gypsum board. At present, except for a small amount of titanium gypsum used as cement retarder, most of it is in a stacking state, with a comprehensive utilization rate of less than 10%, and at the same time causing waste of land resources and high maintenance costs.
[0003] There are some comprehensive utilization technologies of titanium gypsum disclosed in the prior art, such as calcining titanium gypsum in a reducing atmosphere to prepare calcium oxide and sulfur dioxide, which goes through the steps of gypsum → reducing atmosphere → decomposition and calcination → cooling and grinding → cement preparation → drying and absorption of calcination kiln exhaust gas → conversion → finished sulfuric acid. The processing process is complicated, the temperature is high, and the operation is cumbersome.
[0004] In addition, in the sulfuric acid method of titanium dioxide process, some other by-products are also produced, such as ferrous yellow produced after waste acid treatment. Ferrous yellow has a high content of free sulfuric acid and is a hazardous solid waste, which is difficult to treat. Summary of the invention
[0005] In view of the above-mentioned defects in the prior art, the present invention provides a method for resource utilization of titanium gypsum, and the specific scheme is:
[0006] A method for resource utilization of titanium gypsum, comprising the following steps:
[0007] 1) Mix the yellow ferrous iron produced as a by-product in the sulfuric acid process with titanium gypsum for slurrying, add fluorine-containing wastewater during slurrying, and control the pH value of the slurry to be 2.8-4.1;
[0008] 2) The slurry is subjected to solid-liquid separation to obtain recovered gypsum and a primary solution; the primary solution is used to prepare ferrous sulfate heptahydrate or polyferric sulfate.
[0009] The present invention mixes titanium gypsum with another byproduct yellow ferrous iron in the sulfuric acid method titanium dioxide process for pulping, and uses free sulfuric acid in the yellow ferrous iron to neutralize ferrous hydroxide and ferric hydroxide in the titanium gypsum, so that the iron in the titanium gypsum slurry is completely converted into ferric sulfate salt, which is dissolved in the liquid phase with ferrous sulfate to form a solution, and the total iron content of the solution is about 7%-9%. After solid-liquid separation, low-iron calcium sulfate dihydrate is obtained, at which the iron content in the gypsum is about 0.5%, the gypsum is white or light yellow, and the iron removal rate in the titanium gypsum is about 90%, thereby improving the quality of the titanium gypsum.
[0010] When the pH value is higher than 4.1, the solubility of ferrous hydroxide and ferric hydroxide is low, and the obtained titanium gypsum is yellowish in color and cannot meet the recycling requirements. When the pH value is lower than 2.8, the titanium in the titanium gypsum is acid-lyzed into the solution, which increases the difficulty of preparing ferrous sulfate heptahydrate or polyferric sulfate in the primary solution.
[0011] In the present invention, the titanium gypsum used for slurrying can be stockpiled solid titanium gypsum, or can be neutralized slurry formed after neutralization of acidic wastewater.
[0012] Since calcium sulfate is slightly soluble in water, a trace amount of calcium sulfate is dissolved in the primary solution formed after solid-liquid separation, which affects the quality of the subsequent preparation of ferrous sulfate heptahydrate and polyferric sulfate.
[0013] In view of the technical problem, the present invention provides an improved method, wherein in step 1), fluorine-containing wastewater is added during mixing and beating; in step 2), a precipitant containing phosphate is added to the primary solution to form calcium fluorophosphate precipitation, and solid-liquid separation is performed after flocculation to obtain a secondary solution, which is then used to prepare ferrous sulfate heptahydrate or polyferric sulfate. The precipitant can be ammonium hydrogen phosphate.
[0014] Calcium fluorophosphate has very low solubility in water. This method can further remove calcium from the primary solution and improve the quality of subsequent preparation of ferrous sulfate heptahydrate and polyferric sulfate.
[0015] Preferably, the amount of fluorine-containing wastewater and precipitant added is based on the nCa content in the solution. 2+ :nPO4 3- :nF - =20:3:1. According to this ratio, a molecular formula of Ca 10 Stable precipitation of (PO4)6F2.
[0016] Preferably, Al(OH)3 is added to the primary solution to control the pH to 6-8. The amount of Al(OH)3 added is based on the amount of nCa in the solution. 2+ :nPO4 3- :nF - :nAl 3+=20:3:1:6 to 10. In this range, the removal effect of calcium and fluoride in the primary solution can be further improved.
[0017] Preferably, the fluorine-containing wastewater is wastewater generated by cleaning filter cloth in a sulfuric acid process for producing titanium dioxide.
[0018] In the sulfuric acid method of titanium dioxide process, silica will be deposited on the filter cloth used for filtering titanic acid, and fluorine-containing wastewater will be produced after cleaning with hydrofluoric acid. This method utilizes the fluorine-containing wastewater for pulping and solves the problem of treating the fluorine-containing wastewater at the same time.
[0019] The method of the invention utilizes free sulfuric acid in ferrous iron to neutralize titanium gypsum, and at the same time realizes the recycling of calcium iron resources, thus solving the problem of environmental damage caused by the stacking of two solid wastes.
[0020] In addition, in the improved method, the fluorine-containing wastewater in the sulfuric acid method titanium dioxide process is further utilized to improve the purity of the recovered iron-containing solution and solve the problem of treating the fluorine-containing wastewater.
[0021] The present invention realizes waste treatment by waste in the sulfuric acid method titanium dioxide process, has low investment cost and simple process, solves the storage problem of various hazardous wastes, and realizes the recycling of resources, and has high promotion value. DETAILED DESCRIPTION
[0022] The present invention is described in detail below in conjunction with the embodiments of the present invention. The description herein is only used to explain the present invention, but is not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work, any modifications, equivalent substitutions, improvements, etc., should be included in the protection scope of the present invention.
[0023] Example
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0025] Embodiment 1:
[0026] 165g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 2.8. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was white.
[0027] Embodiment 2:
[0028] 149g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 3.2. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was white.
[0029] Embodiment 3:
[0030] 136 yellow ferrous iron and 100g titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 3.6. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was white.
[0031] Embodiment 4:
[0032] 123g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 4.1. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was white.
[0033] Embodiment 5:
[0034] 147g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried. Fluorine-containing wastewater was produced after washing with a metatitanic acid filter cloth. The pH value of the slurry was 3.6. The slurry was filtered to separate the filter cake and the primary solution. The filter cake was washed with water to obtain white recycled gypsum. Diammonium hydrogen phosphate was added to the primary solution. nCa in the solution 2+ :nPO4 3- :nF - =20:3:1, pH value is 4.2. Add a small amount of flocculant and filter to obtain a secondary solution.
[0035] Embodiment 6:
[0036] 147g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried. Fluorine-containing wastewater was generated after washing with a metatitanic acid filter cloth. The pH value of the slurry was 3.6. The slurry was filtered to separate the filter cake and the primary solution. The filter cake was washed with water to obtain white recycled gypsum. Diammonium hydrogen phosphate and aluminum hydroxide were added to the primary solution. nCa 2+ :nPO4 3- :nF - :nAl 3+ =20:3:1:6, pH value is 6. Add a small amount of flocculant and filter to obtain a secondary solution.
[0037] Embodiment 7:
[0038] 147g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried. Fluorine-containing wastewater was generated after washing with a metatitanic acid filter cloth. The pH value of the slurry was 3.6. The slurry was filtered to separate the filter cake and the primary solution. The filter cake was washed with water to obtain white recycled gypsum. Diammonium hydrogen phosphate and aluminum hydroxide were added to the primary solution. nCa 2+ :nPO4 3- :nF - :nAl 3+=20:3:1:10, pH value is 7. Add a small amount of flocculant and filter to obtain a secondary solution.
[0039] Embodiment 8:
[0040] 147g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried. Fluorine-containing wastewater was produced after washing with a metatitanic acid filter cloth. The pH value of the slurry was 3.6. The slurry was filtered to separate the filter cake and the primary solution. The filter cake was washed with water to obtain white recycled gypsum. Diammonium hydrogen phosphate and aluminum hydroxide were added to the primary solution, and the pH value was 9. A small amount of flocculant was added for filter pressing to obtain a secondary solution.
[0041] Comparative Example 1:
[0042] 182g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 2.4. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was white.
[0043] Comparative Example 2:
[0044] 111g of yellow ferrous iron and 100g of titanium gypsum were mixed and slurried, and clean water was used for slurrying, and the pH value of the slurry was 4.5. The slurry was filtered to separate the filter cake and the primary solution, and the filter cake was washed with water, and the recovered gypsum was light yellow.
[0045] The titanium and calcium contents of the primary solutions obtained in Examples 1-4 and Comparative Examples 1-2 were tested, and the titanium, calcium and fluorine contents of the secondary solutions obtained in Examples 5-8 were tested. The comparison results are as follows:
[0046] Titanium content in solution Calcium content in solution Fluoride content in solution Example 1 0.52% 0.26% - Example 2 0.03% 0.25% - Example 3 0.01% 0.23% - Example 4 0.01% 0.26% - Example 5 0.01% 0.12% 13ppm Example 6 0.01% 0.07% 1.5ppm Example 7 0.01% 0.11% 2ppm Example 8 0.01% 0.13% 15ppm Comparative Example 1 0.61% 0.27% - Comparative Example 2 0.01% 0.32% -
[0047] The recycled gypsum obtained in Example 2 is yellowish, and the control of pH value during mixed pulping has a great influence on the removal effect of iron in titanium gypsum, as well as the titanium content in the primary solution. The calcium content in the secondary solution can be reduced by pulping with fluorine-containing wastewater and adding phosphorus to form calcium fluorophosphate precipitation, and the precipitation effect can be further improved by compounding aluminum hydroxide and controlling the pH of the secondary solution.
[0048] The products of ferrous sulfate recovery generally have relatively high purity requirements, such as battery-grade ferrous sulfate heptahydrate and polyferric sulfate for water purifier. Therefore, a ferrous sulfate product with higher purity can be prepared by treating according to the methods of Implementation 6 and Example 7.
Claims
1. A method for resource utilization of titanium gypsum, characterized in that: The following steps are involved: 1) Mix the yellow ferrous iron produced as a by-product in the sulfuric acid process with titanium gypsum for slurrying, add fluorine-containing wastewater during slurrying, and control the pH value of the slurry to be 2.8-4.1; 2) The slurry is subjected to solid-liquid separation to obtain recovered gypsum and a primary solution; the primary solution is used to prepare ferrous sulfate heptahydrate or polyferric sulfate; In step 2), a precipitant containing phosphate is added to the primary solution, and Al(OH)3 is also added to the primary solution to control the pH to 6-7. The amount of addition is based on the nCa content of the solution. 2+ :nPO4 3- :nF - :nAl 3+ =20:3:1:6~10 to control; forming calcium fluorophosphate precipitation, flocculation and solid-liquid separation to obtain a secondary solution, the secondary solution is then used to prepare ferrous sulfate heptahydrate or polyferric sulfate.
2. The method for resource utilization of titanium gypsum according to claim 1, characterized in that: The fluorine-containing wastewater is wastewater generated by cleaning filter cloth in the sulfuric acid process of titanium dioxide.