A wear-resistant PA composition and its preparation method and application
Through the reaction of specific epoxy resin with the end amino group of PA66 and the combination of antioxidants, a cross-linked structure is formed, which solves the problem of wear-resistant nylon materials under the action of high heat and lubricants, and realizes the wear-resistant performance attenuation under high temperature conditions. Good wear resistance and mechanical performance stability meet the needs of industries such as high-speed rail and passenger cars.
Patent Information
- Application Number
- CN202310480683.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The existing wear-resistant nylon materials are prone to attenuation under high heat and lubricant conditions, and have poor mechanical properties and are unable to meet the needs of high-speed rail, passenger cars and other industries.
By selecting a specific epoxy value, the epoxy resin reacts with the end amino group of PA66 to form a crosslinked structure, combining antioxidants and PTFE, the penetration of grease components is reduced, and the wear resistance and mechanical stability of the PA composition is improved.
After the lubricating ester resistance test at 1000h and 140°C, the PA composition maintained good wear resistance and mechanical properties, the tensile strength retention rate reached more than 87%, the bending strength retention rate reached more than 84%, and the wear amount did not exceed 2.5. Significantly improves performance under high temperature grease.
Smart Images

Figure BDA0004207041160000021 
Figure BDA0004207041160000022 
Figure BDA0004207041160000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer compound compositions, and more specifically, to a wear-resistant PA composition and a preparation method and application thereof. Background Art
[0002] Polyamide 66 material (PA66) is widely used in the fields of electronics, rail transit, power tools, home appliances, sports equipment, etc. due to its excellent heat resistance, solvent resistance, mechanical and processing properties. Especially in the field of rail transit technology, bearings are indispensable components, and the bearing cage in the bearing component can isolate and retain the rolling elements. Moreover, during the operation of the bearing, the cage will be subjected to great centrifugal force, impact and vibration, and will also generate a lot of heat due to friction, which puts forward higher mechanical, wear and heat resistance requirements for the performance of the bearing cage. In addition, the bearing cage must also withstand the effects of chemical media, such as lubricants, lubricant additives, organic solvents and coolants, so there are also high requirements for the solvent resistance of the cage.
[0003] Currently, most commonly used non-metallic bearing retainers are made of nylon, phenolic tape, polytetrafluoroethylene and other materials. Among them, nylon material has been widely used due to its balanced advantages in heat resistance, mechanics, wear resistance and cost. However, ordinary nylon will experience significant performance degradation under the conditions of high heat and lubricating ester, and cannot meet the use requirements of high-speed rail, passenger car and other industries.
[0004] For example, the prior art discloses a physicochemically synergistically modified low-temperature, high-strength, wear-resistant nylon 66 and a preparation method thereof. The material comprises PA66, epoxy resin, antioxidant, wear-resistant agent, lubricant and glass fiber, so that under the shearing and heat action of the screw, PA66 and the epoxy resin further melt and react to modify PA66, and at the same time, the modified PA66 is reacted with the wear-resistant agent, lubricant and antioxidant to obtain the physicochemically synergistically modified low-temperature, high-strength, wear-resistant nylon 66. The material has good strength and wear resistance at a low temperature of -50°C, but cannot solve the problems of attenuation of wear resistance and poor stability of mechanical properties under high heat and lubricant conditions. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects and shortcomings of existing wear-resistant nylon materials, such as easy attenuation of wear resistance and poor stability of mechanical properties under high heat and lubricant conditions, and to provide a wear-resistant PA composition.
[0006] Another object of the present invention is to provide a method for preparing the wear-resistant PA composition.
[0007] Another object of the present invention is to provide use of the wear-resistant PA composition in preparing bearing components.
[0008] Another object of the present invention is to provide a bearing retainer material.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] The present invention protects a wear-resistant PA composition, which comprises the following components by weight:
[0011]
[0012] The epoxy value of the epoxy resin is 0.02 to 0.4; the terminal amino group content of the PA66 resin measured according to the HG / T 4182-2012 standard is ≥40 mmol / kg.
[0013] The present invention selects an epoxy resin with a specific epoxy value to react with the terminal amino group of PA66 to form a cross-linked structure to reduce the permeability of the PA composition to reduce the penetration of the grease component, and is combined with an antioxidant to effectively reduce the degradation of PA66 by high-temperature environment and grease, so that after the PA66 resin is combined with PTFE, the lubrication and wear resistance of PTFE can be fully exerted, thereby giving the PA composition excellent wear resistance and mechanical property stability under the action of high-temperature grease.
[0014] Among them, the epoxy value of the epoxy resin and the terminal amino content of PA66 jointly affect the transmittance of the wear-resistant PA composition. When the epoxy value of the epoxy resin is less than 0.02 or the terminal amino content of PA66 is less than 40mmol / kg, the epoxy resin and the terminal amino group of nylon do not react sufficiently, and it is difficult to effectively reduce the degradation of the nylon resin. Moreover, when the amount of epoxy resin added is too high, it will also cause injection molding abnormalities such as phase separation, and the retention rate improvement effect is not good. When the epoxy value of the epoxy resin is greater than 0.4, the fluidity of the PA composition will decrease, the processing will be difficult, and the impact performance of the PA composition will decrease due to excessive cross-linking.
[0015] The epoxy value of the above epoxy resin can be measured by the hydrochloric acid acetone method (GB1677).
[0016] Specifically, the reinforcing fiber can be one or more of glass fiber, carbon fiber, metal fiber, plant fiber and mineral fiber. Preferably, the reinforcing fiber is glass fiber.
[0017] Preferably, the wear-resistant PA composition comprises the following components in parts by weight:
[0018]
[0019] In a specific implementation manner, the PA66 resin has a terminal amino group content of 40.2 to 82 mmol / kg as measured according to HG / T 4182-2012 standard; and / or the epoxy value of the epoxy resin is 0.25 to 0.4.
[0020] Specifically, the terminal amino group content of the PA66 resin measured according to the HG / T 4182-2012 standard is 40.2-82 mmol / kg, and optionally, the terminal amino group content is 40.7-49.2 mmol / kg.
[0021] Optionally, the epoxy value of the epoxy resin is 0.23, 0.25, 0.3, 0.35, or 0.4; preferably, the epoxy value of the epoxy resin is 0.25 to 0.4.
[0022] Specifically, the epoxy resin is bisphenol A epoxy resin.
[0023] Optionally, the relative viscosity of the PA66 resin measured according to ISO 307-2007 standard is 2.1-2.7; preferably, the relative viscosity of the PA66 resin is 2.4-2.7.
[0024] Preferably, the antioxidant is one or more of a hindered phenol antioxidant, a hindered amine antioxidant and a phosphite antioxidant.
[0025] The present invention also protects a method for preparing the above-mentioned wear-resistant PA composition, comprising the following steps:
[0026] PA66 resin, PTFE, epoxy resin and antioxidant are added to the twin-screw extruder from the main feeding port, and the reinforcing fiber is added to the twin-screw extruder from the side feeding port. After being evenly mixed, they are melt-extruded and granulated to obtain a wear-resistant PA composition.
[0027] Specifically, the temperature of the melt extrusion is 190°C to 275°C.
[0028] The use of the above-mentioned wear-resistant PA composition in the preparation of bearing components is also within the protection scope of the present invention.
[0029] The present invention also protects a bearing retainer material comprising the wear-resistant PA composition.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The wear-resistant PA composition of the present invention reduces the permeability of the PA composition to reduce the penetration of grease components by selecting an epoxy resin with a specific epoxy value to react with the end group of PA66. The wear-resistant PA composition can be matched with an antioxidant to effectively reduce the degradation of PA66, so that after the PA66 resin is combined with PTFE, the lubrication and wear resistance of PTFE can be fully exerted, so that the PA composition still has good wear resistance and mechanical properties after a 1000h, 140°C grease resistance test. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0033] 1. Raw materials and reagents
[0034] PA66 resin 1, terminal amino content is 40.7mmol / kg, its relative viscosity is 2.7 according to ISO 307-2007 standard, brand PA66 EPR27, manufacturer Henan Shenma;
[0035] PA66 resin 2, terminal amino content is 40.2mmol / kg, its relative viscosity is 2.4 according to ISO 307-2007 standard, brand PA66 EPR24, manufacturer Henan Shenma;
[0036] PA66 resin 3, terminal amino content is 49.2mmol / kg, its relative viscosity is 2.4 according to ISO 307-2007 standard, brand PA6624FE2K, manufacturer Rhodia;
[0037] PA66 resin 4, terminal amino content is 82mmol / kg, its relative viscosity is 2.7 according to ISO 307-2007 standard, brand PA66 EP-158NH, manufacturer Huafeng Group
[0038] PA66 resin 5, terminal amino content is 38mmol / kg, its relative viscosity is 2.7 according to ISO 307-2007 standard, brand PA66 50BWFS, manufacturer Ascend;
[0039] Epoxy resin A1: bisphenol A epoxy resin, E-20, epoxy value 0.2, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0040] Epoxy resin A2: bisphenol A epoxy resin, E-06, epoxy value 0.04, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0041] Epoxy resin A3: bisphenol A epoxy resin, E-10, epoxy value 0.08, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0042] Epoxy resin A4: bisphenol A epoxy resin, E-14, epoxy value 0.1, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0043] Epoxy resin A5: bisphenol A epoxy resin, CYD-134, epoxy value 0.38, manufacturer Sinopec;
[0044] Epoxy resin A6: bisphenol A epoxy resin, E-44, epoxy value 0.4, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0045] Epoxy resin A7: bisphenol A epoxy resin, E-51, epoxy value 0.51, manufacturer Wuxi Bluestar Petrochemical Co., Ltd.
[0046] Polypropylene glycol diglycidyl ether, commercially available;
[0047] Antioxidant 1: Antioxidant 1098, molecular weight 637, manufacturer BASF;
[0048] Antioxidant 2: Antioxidant 1790, molecular weight 700, manufacturer Solvay;
[0049] Antioxidant 3: Sumisorb 400, molecular weight 438, manufacturer Shanghai Yasuda Chemical Co., Ltd.
[0050] PTFE: Brand F-5AEX, manufacturer Solvay;
[0051] The reinforcing fiber is glass fiber, brand ECS10-03-568H, manufacturer China Jushi Co., Ltd.
[0052] 2. The wear-resistant PA compositions of the embodiments and comparative examples of the present invention are prepared by the following preparation method:
[0053] After weighing each component according to the formula and mixing them evenly, the components are added into a twin-screw extruder for melt blending and extrusion granulation to obtain a thin-walled, highly light-transmitting, flame-retardant nylon composite material;
[0054] Among them, the glass fiber is added from the side feeding port of the twin-screw extruder, and the melt extrusion conditions of the twin-screw extruder are: the temperature of zone one is 190°C, the temperature of zone two is 260°C, the temperature of zone three is 270°C, the temperature of zone four is 275°C, the temperature of zone five is 275°C, the temperature of zone six is 270°C, the temperature of zone seven is 270°C, the temperature of zone eight is 270°C, the temperature of zone nine is 270°C, and the main engine speed is 400r / min.
[0055] 3. Performance testing
[0056] (1) Lubricating grease wear test: The test specimens were first completely immersed in lubricating grease (the lubricating grease was commercially available for Type IV rolling bearing lubricating grease for railway vehicles), and then placed in an oven at 140°C for 1000 h before a wear test. The wear test was conducted in accordance with the test standard of GBT 3960-2016, with a load of 5 kN and a test of 1000 h.
[0057] (2) Performance retention rate test: The test specimens were randomly divided into two batches, and the tensile strength and bending strength of one batch of specimens were first tested; then the other batch of specimens were completely immersed in lubricating grease (the lubricating grease was type IV railway vehicle rolling bearing lubricating grease, commercially available), and then placed in an oven at 140°C for 1000 hours for tensile strength and bending strength tests; then, based on the tensile strength and bending strength of the specimens before and after the high-temperature grease test, the performance retention rate was calculated, performance retention rate = performance after high-temperature grease test / performance before high-temperature grease test*100%; the above tensile strength was tested according to ISO 527-2012 standard, and the bending strength was tested according to ISO 178-2019 standard.
[0058] Examples 1 to 15
[0059] The weight proportions of the components of the wear-resistant PA compositions in Examples 1 to 15 are shown in Tables 1 and 2.
[0060] Table 1 Wear-resistant PA compositions in Examples 1 to 11
[0061]
[0062]
[0063] Table 2 Wear-resistant PA compositions in Examples 12 to 15
[0064]
[0065] Comparative Examples 1 to 5
[0066] The weight proportions of the components in the wear-resistant PA compositions in Comparative Examples 1 to 5 are shown in Table 3.
[0067] Table 3 Wear-resistant PA compositions in Comparative Examples 1 to 5
[0068]
[0069]
[0070] The performance test results of the wear-resistant PA compositions in the embodiments and comparative examples according to the above-mentioned method are shown in Table 4.
[0071] Table 4 Test results of various embodiments and comparative examples
[0072]
[0073] It can be seen from the data in Table 4 that the PA composition of the present invention still maintains a good mechanical property retention rate after the 1000h, 140°C lubricating ester resistance test, wherein the tensile strength retention rate is maintained at more than 87%, the bending strength retention rate is maintained at more than 84%, and it also has good wear resistance, with the wear amount not exceeding 2.5, and further, the wear amount is only 1.4 to 2.5; from Comparative Example 1, it can be found that when the epoxy value of the epoxy resin is greater than 0.4, the wear amount of the PA composition increases after the lubricating ester resistance test. It can be seen from Comparative Examples 2 and 3 that when the epoxy resin is added too much, it is easy to cause injection molding abnormalities such as phase separation and cannot be extruded; and when the epoxy resin is added too little, the epoxy resin and the PA66 resin do not react sufficiently, the nylon resin is severely degraded, and it is difficult to effectively improve the wear resistance of the PA composition.
[0074] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A wear-resistant PA composition, It is characterized in that By weight, it includes the following components: 40-80 parts of PA66 resin; PTFE 0-15 parts; 10-50 parts of reinforcing fiber; 1 to 5 parts of epoxy resin; 0.1 to 3 parts of antioxidant; The epoxy value of the epoxy resin is 0.2 to 0.4, and the epoxy resin is a bisphenol A epoxy resin; the terminal amino content of the PA66 resin measured according to the HG / T 4182-2012 standard is 40 to 82 mmol / kg, and the relative viscosity of the PA66 resin measured according to the ISO307-2007 standard is 2.1 to 2.7; The antioxidant is one or more of a hindered phenol antioxidant, a hindered amine antioxidant and a phosphite antioxidant.
2. The wear-resistant PA composition according to claim 1, It is characterized in that By weight, it includes the following components: 60-80 parts of PA66 resin; PTFE 3-10 parts; 15-40 parts of reinforcing fiber; 1 to 3 parts of epoxy resin; Antioxidant 0.2 to 2 parts.
3. The wear-resistant PA composition according to claim 1, It is characterized in that The PA66 resin has a terminal amino group content of 40.2 to 82 mmol / kg as measured according to HG / T4182-2012 standard; and / or the epoxy value of the epoxy resin is 0.25 to 0.
4.
4. A method for preparing the wear-resistant PA composition according to any one of claims 1 to 3, It is characterized in that The following steps are involved: PA66 resin, PTFE, epoxy resin and antioxidant are added into the extruder from the main feeding port, and reinforcing fiber is added into the extruder from the side feeding port. After mixing, the mixture is melt-extruded and granulated to obtain a wear-resistant PA composition.
5. The method for preparing the wear-resistant PA composition according to claim 4, It is characterized in that The temperature of the melt extrusion is 190°C to 275°C.
6. Use of the wear-resistant PA composition according to any one of claims 1 to 3 in the preparation of bearing components.
7. A bearing cage material, It is characterized in that The bearing retainer material comprises the wear-resistant PA composition according to any one of claims 1 to 3.