Polyimide film for graphite sheet, method for producing the same, and graphite sheet produced therefrom
By adding a sublimative inorganic filler to the polyimide film and adopting a specific manufacturing method, the problem of structural damage in the heat treatment process of high-thickness graphite sheets is solved, and the excellent thermal conductivity and surface quality of high-thickness graphite sheets are achieved.
Patent Information
- Application Number
- CN202180077401.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-11-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The prior art is difficult to keep the surface smooth and the internal structure of graphite sheets when manufacturing high-thickness graphite sheets during heat treatment, mainly due to the generation of sublimation gas, resulting in surface and internal structure damage.
A polyimide film having a thickness of 100 μm or more is used, and a sublimative inorganic filler, such as calcium hydrogen phosphate and barium sulfate, is added therein. By a specific manufacturing method, it includes reacting in a solvent to form a polyamic acid solution and adding anis The amination agent and the dehydrating agent are coated and dried and heat-treated to form a graphite sheet with excellent thermal conductivity.
The manufacturing of high-thick graphite sheets is achieved, ensuring excellent surface quality and thermal conductivity, reducing structural damage during carbonization and graphitization, and improving the flexibility and moldability of graphite sheets.
Smart Images

Figure BDA0004232460710000111
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide film for a graphite sheet, a method for producing the same, and a graphite sheet produced therefrom. More specifically, the present invention relates to a polyimide film for a graphite sheet having excellent surface quality and thermal conductivity and capable of ensuring a high thickness, a method for producing the same, and a graphite sheet produced therefrom. Background Art
[0002] Recent electronic devices have become lighter, smaller, thinner, and more highly integrated, so a lot of heat is generated in electronic devices. Such heat may shorten the life of the product or cause malfunctions, false start-ups, etc. Therefore, thermal management of electronic devices has become an important issue.
[0003] Graphite sheets have higher thermal conductivity than metal sheets such as copper and aluminum, and therefore have attracted attention as heat dissipation components for electronic devices. In particular, active research is being conducted on thick graphite sheets (e.g., graphite sheets with a thickness of about 100 μm or more) that are more advantageous in terms of heat capacity than thin graphite sheets (e.g., graphite sheets with a thickness of about 40 μm or less).
[0004] Graphite sheets can be produced by various methods, for example, by carbonizing and graphitizing polymer films. In particular, polyimide films have attracted attention as polymer films for producing graphite sheets due to their excellent mechanical, thermal dimensional stability, chemical stability, etc.
[0005] A high-thickness graphite sheet can be manufactured by carbonizing and graphitizing a high-thickness polyimide film (e.g., a polyimide film having a thickness of about 100 μm or more), but there is a problem of difficulty in obtaining a high-quality graphite sheet with a smooth surface and an undamaged internal graphite structure during the heat treatment process, and the yield is low. It is speculated that this is because, assuming that the surface layer and the interior of the polyimide film are carbonized and graphitized almost simultaneously, in the case of a high-thickness polyimide film, the amount of sublimation gas generated from the interior is large, and the possibility of damage to the graphite structure formed or being formed on the surface layer is high. In addition, not only the surface, but also the pressure of the central part of the film and the inner side adjacent thereto will be greatly increased due to a large amount of sublimation gas, thereby damaging the graphite structure formed or being formed, which can also be regarded as one of the reasons.
[0006] Therefore, the reality is that there is a great need for technology that can produce high-quality graphite sheets with high thickness and good surface quality and graphite structure. Summary of the invention
[0007] Technical issues
[0008] An object of the present invention is to provide a polyimide film for a graphite sheet which has excellent surface quality and thermal conductivity and can ensure a high thickness.
[0009] Another object of the present invention is to provide a method for producing the polyimide film.
[0010] Another object of the present invention is to provide a graphite sheet produced from the polyimide film.
[0011] Methods for solving problems
[0012] 1. According to one aspect, a polyimide film for a graphite sheet is provided. The polyimide film may have a thickness of 100 μm or more, and a 1 wt % loss thermal decomposition temperature measured by thermogravimetric analysis (TGA) may be 480° C. or less.
[0013] 2. According to another aspect, a polyimide film for a graphite sheet is provided. The polyimide film may have a thickness of 100 μm or more, and an L* value measured by a colorimeter may be 40 or more.
[0014] 3. In the first or second embodiment, the polyimide film may contain a sublimable inorganic filler.
[0015] 4. In the third embodiment, the average particle size (D 50 ) may be 1 μm to 10 μm, and the content of the sublimable inorganic filler may be 0.15 to 0.25 parts by weight per 100 parts by weight of the polyimide film.
[0016] 5. In the third or fourth embodiment, the sublimable inorganic filler may include calcium hydrogen phosphate, barium sulfate, calcium carbonate, or a combination thereof.
[0017] 6. According to another aspect, a method for producing a polyimide film for a graphite sheet is provided. The method may include the following steps: reacting a diamine monomer and a dianhydride monomer in a solvent to produce a polyamic acid solution; adding an imidizing agent, a dehydrating agent, a sublimable inorganic filler, or a combination thereof to the polyamic acid solution to produce a precursor composition for a polyimide film; coating the precursor composition on a support and drying it to produce a gel film; and heat-treating the gel film to produce any one of the polyimide films in the first to fifth embodiments.
[0018] 7. In the sixth embodiment, the diamine monomer may include 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane or a combination thereof, and the dianhydride monomer may include pyromellitic acid dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,3,3',4-biphenyltetracarboxylic acid dianhydride, oxydiphthalic anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride or a combination thereof.
[0019] 8. In the sixth or seventh embodiment, the drying may be performed at 30° C. to 200° C. for 15 seconds to 30 minutes.
[0020] 9. In any one of the sixth to eighth embodiments, the heat treatment may be performed at 250° C. to 450° C. for 30 seconds to 40 minutes.
[0021] 10. According to another aspect, a graphite sheet is provided. The graphite sheet is formed by carbonizing and graphitizing any one of the polyimide films of the first to fifth embodiments or a polyimide film manufactured by any one of the manufacturing methods of the sixth to ninth embodiments, and may have a thickness of 100 μm or more.
[0022] 11. In the tenth embodiment, the thermal diffusion coefficient of the graphite sheet can be 640 mm 2 / s or more.
[0023] 12. In the tenth or eleventh embodiment, the number of protrusions (bright spots) having a major diameter of 0.05 mm or more per unit area of 50 mm x 50 mm of the graphite sheet is 5 or less.
[0024] Effects of the Invention
[0025] The present invention has the effect of providing a polyimide film for a graphite sheet which is excellent in surface quality and thermal conductivity and can ensure a high thickness, a method for producing the same, and a graphite sheet produced therefrom. DETAILED DESCRIPTION
[0026] Best Mode for Carrying Out the Invention
[0027] In this specification, an expression in the singular includes an expression in the plural unless the context clearly dictates otherwise.
[0028] In this specification, the terms including or having mean that the features or components described in the specification are present, and do not exclude the possibility of adding one or more other features or components in advance.
[0029] When interpreting constituent elements, even if there is no particular explicit description, they should be interpreted in a manner including a range of error.
[0030] In the present specification, “to” in “a to b” indicating a numerical range is defined as ≥a and ≤b.
[0031] The inventors of the present invention have conducted intensive research on a polyimide film for a graphite sheet having excellent surface quality and thermal conductivity and capable of ensuring a high thickness. As a result, they have found that, when a graphite sheet is formed from a polyimide film having a thickness of 100 μm or more, a 1 wt% loss thermal decomposition temperature of 480° C. or less as measured by thermogravimetric analysis (TGA), and / or an L* value of 40 or more as measured by a colorimeter, the time required for carbonization and / or graphitization can be shortened, resulting in the manufacture of a high-thickness graphite sheet having excellent surface quality and thermal conductivity, thereby completing the present invention.
[0032] Hereinafter, the present invention will be described in further detail.
[0033] Polyimide film for high thickness graphite sheet
[0034] The thickness of the polyimide film of one aspect of the present invention may be 100 μm or more, and the 1 wt% loss thermal decomposition temperature measured by thermogravimetric analysis (TGA) may be 480°C or less (e.g., 300°C to 480°C, and for example, 400°C to 480°C). Within the above range, a high-thickness graphite sheet with excellent surface quality and thermal conductivity can be manufactured. Here, thermogravimetric analysis (TGA) can be measured using a thermogravimetric analyzer (TGA 5500, TA Company) at a heating rate of 10°C / min from room temperature (23°C) to 1,100°C, but is not limited thereto. For example, the 1 wt% loss thermal decomposition temperature of the polyimide film measured by thermogravimetric analysis (TGA) may be 460°C or less, and for example, 450°C or less, and for example, 440°C or less, and for example, 430°C or less. Within the above range, it is more conducive to the manufacture of a high-thickness graphite sheet with excellent surface quality and thermal conductivity, but is not limited thereto.
[0035] The thickness of the polyimide film in another aspect of the present invention can be 100 μm or more, and the L* value measured by a colorimeter can be 40 or more. Within the above range, a high-thickness graphite sheet with excellent surface quality and thermal conductivity can be manufactured. Here, the L* value can be measured using a colorimeter (Ultra scan pro, Hunter Lab). For example, the L* value of the polyimide film measured by a colorimeter can be 45 or more, and for example, it can be 50 or more, and for example, it can be 53 or more. Within the above range, it can be more conducive to the manufacture of a high-thickness graphite sheet with excellent surface quality and thermal conductivity, but is not limited thereto.
[0036] According to one embodiment, the thickness of the polyimide film can be 100 μm to 200 μm (for example, 100 μm to 170 μm, for example 100 μm to 170 μm, for example 100 μm to 150 μm). Within the above range, it can be more conducive to the manufacture of high-thickness graphite sheets with excellent surface quality and thermal conductivity, but is not limited to this.
[0037] According to one embodiment, the polyimide film may contain a sublimable inorganic filler. The so-called "sublimable inorganic filler" refers to an inorganic filler that sublimates due to heat during the carbonization and / or graphitization process when manufacturing a graphite sheet. In the case where the polyimide film contains a sublimable inorganic filler, pores can be formed in the graphite sheet by means of the gas generated by the sublimation of the sublimable inorganic filler during the manufacture of the graphite sheet. Therefore, the exhaust of the sublimated gas generated when manufacturing the graphite sheet proceeds smoothly and a high-quality graphite sheet can be obtained. Not only that, the flexibility of the graphite sheet can also be improved, and ultimately the operability and formability of the graphite sheet can be improved. Examples of sublimable inorganic fillers include calcium hydrogen phosphate, barium sulfate, calcium carbonate, etc., but are not limited to these. The average particle size (D 50 ) can be 1 μm to 10 μm (e.g., 1 μm to 5 μm), and within the above range, it is possible to obtain an excellent graphite sheet, but it is not limited thereto. Based on 100 parts by weight of the polyimide film, the content of the sublimable inorganic filler can be 0.15 parts by weight to 0.25 parts by weight (e.g., 0.2 parts by weight to 0.25 parts by weight), and within the above range, it is possible to obtain an excellent graphite sheet, but it is not limited thereto.
[0038] The polyimide film can be manufactured without limitation using a common method known in the field of polyimide films. For example, the polyimide film can be manufactured by the following steps: a polyamic acid solution is manufactured by reacting a diamine monomer and a dianhydride monomer in a solvent; an imidizing agent, a dehydrating agent, a sublimable inorganic filler or a combination thereof is added to the polyamic acid solution to manufacture a precursor composition for a polyimide film; the precursor composition is coated on a support and dried to manufacture a gel film; and the gel film is heat-treated to manufacture a polyimide film.
[0039] First, a polyamic acid solution can be produced by reacting a diamine monomer and a dianhydride monomer in a solvent.
[0040] The solvent is not particularly limited as long as it can dissolve the polyamic acid. For example, the solvent may include an aprotic polar solvent. Examples of aprotic polar solvents include amide solvents such as N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAc); phenolic solvents such as p-chlorophenol and o-chlorophenol; N-methyl-pyrrolidone (NMP), γ-butyrolactone (GBL), diethylene glycol dimethyl ether (Diglyme), etc., which can be used alone or in combination of two or more. Depending on the situation, auxiliary solvents such as toluene, tetrahydrofuran (THF), acetone, methyl ethyl ketone (MEK), methanol, ethanol, and water can also be used to adjust the solubility of polyamic acid.
[0041] As the diamine monomer, various diamine monomers known in the art can be used without limitation within the scope that does not impair the purpose of the present invention. For example, the diamine monomer may include 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, or a combination thereof. In this case, a polyimide film that is favorable for molecular orientation can be formed, thereby being more favorable for forming a graphite sheet with excellent thermal conductivity during carbonization and graphitization.
[0042] As the dianhydride monomer, various dianhydride monomers known in the art can be used without limitation within the scope of not impairing the purpose of the present invention. For example, the dianhydride monomer can include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, oxydiphthalic anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride or a combination thereof, in which case, a polyimide film that is conducive to molecular orientation can be formed, thereby being more conducive to forming a graphite sheet with excellent thermal conductivity during carbonization and graphitization.
[0043] The diamine monomer and the dianhydride monomer are present in the solvent in a substantially equimolar manner, where "substantially equimolar" means that the content of the dianhydride monomer is 99.8 mol% to 100.2 mol% based on the total molar number of the diamine monomer. The method of reacting the diamine monomer and the dianhydride monomer in a substantially equimolar manner can be exemplified by:
[0044] (a) a method in which all diamine monomers (or dianhydride monomers) are added to a solvent, and the dianhydride monomers (or diamine monomers) are added in substantially equimolar amounts to carry out the reaction;
[0045] (b) a method of adding a portion of the diamine monomer (or dianhydride monomer) into a solvent, adding the dianhydride monomer (or diamine monomer) at a ratio of 95 mol% to 105 mol% relative to the diamine monomer (or dianhydride monomer), and then adding the diamine monomer and / or dianhydride monomer in substantially equimolar amounts to carry out a reaction;
[0046] (c) a method in which a portion of diamine monomers (or dianhydride monomers) and a portion of dianhydride monomers (or diamine monomers) are added to a solvent in an excess amount of either one to form a first composition, and a portion of diamine monomers (or dianhydride monomers) and a portion of dianhydride monomers (or diamine monomers) are added to another solvent in an excess amount of either one to form a second composition, and then the first composition and the second composition are mixed and reacted, and in this case, if the diamine monomer (or dianhydride monomer) is excessive in the first composition, the dianhydride monomer (or diamine monomer) is excessive in the second composition. In the above (a) to (c), diamine monomers and dianhydride monomers refer to one or more (e.g., one or two) diamine monomers and dianhydride monomers.
[0047] According to one embodiment, based on 100 parts by weight of the polyamic acid solution, the content of the polyamic acid can be 5 parts by weight to 35 parts by weight. In the above range, the polyamic acid solution can have a molecular weight and viscosity suitable for forming a film. For example, based on 100 parts by weight of the polyamic acid solution, the content of the polyamic acid can be 5 parts by weight to 30 parts by weight, and for example, can be 10 parts by weight to 25 parts by weight, but is not limited thereto.
[0048] According to one embodiment, the polyamic acid solution is heated at 23°C and a shear rate of 1 s -1 The viscosity can be 100,000 cP to 500,000 cP. In the above range, the polyamic acid can have a predetermined molecular weight, and the processability is better when forming a polyimide film. Here, the "viscosity" can be measured using a HAAKE Mars Rheometer. For example, the viscosity of the polyamic acid solution at 23°C and a shear rate of 1s -1 For example, the above mentioned range may be 100,000 cP to 450,000 cP, for example, 150,000 cP to 400,000 cP, for example, 150,000 cP to 350,000 cP, but it is not limited thereto.
[0049] According to one embodiment, the weight average molecular weight of polyamic acid can be 100,000 g / mol to 500,000 g / mol. In the above range, it is more conducive to the manufacture of graphite sheets with excellent thermal conductivity. Here, "weight average molecular weight" can be measured using gel chromatography (GPC) and polystyrene as a standard sample. For example, the weight average molecular weight of polyamic acid can be 100,000 g / mol to 450,000 g / mol, and for example, it can be 150,000 g / mol to 400,000 g / mol, but is not limited thereto.
[0050] Thereafter, an imidizing agent, a dehydrating agent, a sublimable inorganic filler, or a combination thereof may be added to the polyamic acid solution to produce a polyimide film precursor composition. The sublimable inorganic filler has been described above, so its description is omitted.
[0051] The so-called "imidizing agent" is a substance that promotes the ring-closure reaction of polyamic acid. As examples of imidizing agents, aliphatic tertiary amines, aromatic tertiary amines, heterocyclic tertiary amines, etc. can be cited. Among them, from the viewpoint of reactivity as a catalyst, heterocyclic tertiary amines can be used. As examples of heterocyclic tertiary amines, there are quinoline, isoquinoline, β-picoline, pyridine, etc., which can be used alone or in combination of two or more. Relative to 1 mole of amic acid groups in polyamic acid, the addition amount of the imidizing agent can be 0.05 mole to 3 moles (for example, 0.2 mole to 2 moles). When within the above range, sufficient imidization can be achieved, and it can be more conducive to making a film, but is not limited to this.
[0052] The so-called "dehydrating agent" is a substance that promotes the ring-closure reaction by dehydrating the polyamic acid. As examples of dehydrating agents, aliphatic anhydrides, aromatic anhydrides, N, N'-dialkylcarbodiimide, lower aliphatic halides, halogenated lower aliphatic anhydrides, arylphosphonic acid dihalides, thionyl halides, etc. can be cited, and they can be used alone or in combination of two or more. Among them, from the viewpoint of ease of acquisition and cost, aliphatic anhydrides such as acetic anhydride, propionic anhydride, and lactic anhydride can be used. Relative to 1 mole of amic acid groups in polyamic acid, the addition amount of the dehydrating agent can be 0.5 mole to 5 moles (for example, 1 mole to 4 moles). When in the above range, sufficient imidization can be achieved, and it can be more conducive to making a film, but it is not limited to this.
[0053] Thereafter, the precursor composition may be coated on a support and dried to produce a gel film.
[0054] Examples of the support include a glass plate, an aluminum foil, an endless stainless steel belt, and a stainless steel drum, but the support is not limited thereto.
[0055] The coating method is not particularly limited, and for example, a casting method may be used.
[0056] Drying can be performed at 30°C to 200°C for 15 seconds to 30 minutes, for example. Within the above range, it is more advantageous to manufacture the desired polyimide film of the present invention, but the present invention is not limited thereto. According to one embodiment, drying can be performed at 50°C to 150°C for 5 minutes to 20 minutes.
[0057] Depending on the situation, in order to adjust the thickness and size of the finally obtained polyimide film and improve the orientation, the gel film may be further stretched. The stretching may be performed in either the machine direction (MD) or the transverse direction (TD).
[0058] The gel film may then be heat treated to produce a polyimide film.
[0059] The heat treatment can be performed at 250°C to 450°C for 30 seconds to 40 minutes, for example. Within the above range, it is more conducive to the manufacture of the desired polyimide film of the present invention, but it is not limited thereto. The heat treatment can be performed at 250°C (or 300°C or 350°C) to 430°C, for example, 250°C to 420°C, for example, 250°C to 410°C, for example, 250°C to 400°C, for example, 250°C to 390°C for 5 minutes to 30 minutes, for example, 10 minutes to 30 minutes, for example, 15 minutes to 25 minutes. Within the above range, it is more conducive to the manufacture of a high-thickness graphite sheet with excellent surface quality and thermal conductivity, but it is not limited thereto.
[0060] The polyimide film produced by the above production method can contribute to the realization of a graphite sheet having excellent surface quality and thermal conductivity and capable of ensuring a high thickness.
[0061] High thickness graphite sheet
[0062] According to another aspect of the present invention, there is provided a graphite sheet formed by carbonizing and graphitizing the above-mentioned graphite sheet polyimide film. In this case, the thickness of the graphite sheet can be 100 μm or more (e.g., 100 μm to 400 μm), thereby having excellent heat capacity and having characteristics that are advantageous for use as a heat dissipation mechanism used in electronic devices.
[0063] "Carbonization" is a process of forming a primary graphite sheet containing amorphous carbon, non-crystalline carbon and / or amorphous carbon by thermally decomposing the polymer chain of the polyimide film. Carbonization can be carried out, for example, by heating the polyimide film to a temperature in the range of 1,100°C to 1,300°C at a rate of 0.3°C / min to 10°C / min. Within the above range, it is more conducive to the manufacture of high-thickness graphite sheets with excellent surface quality and thermal conductivity, but it is not limited to this. Carbonization can be carried out under reduced pressure or in an inert gas atmosphere. Optionally, in order to achieve high orientation of carbon, pressure can be applied to the polyimide film using a hot press or the like during carbonization. The pressure at this time can be, for example, 5kg / cm 2 Above, for example, it can be 15kg / cm 2 Above, for example, it can be 25kg / cm 2 The above, but not limited to.
[0064] "Graphitization" is a process of rearranging the carbon of amorphous carbon, non-crystalline carbon and / or amorphous carbon to form graphite sheets. Graphitization can be carried out, for example, by heating the primary graphite sheet at a temperature ranging from 2,500°C to 3,000°C at a rate of 0.3°C / min to 20°C / min. Within the above range, it is more conducive to the manufacture of high-thickness graphite sheets with excellent surface quality and thermal conductivity, but it is not limited to this. Graphitization can be carried out under reduced pressure or in an inert gas atmosphere. Optionally, in order to achieve high orientation of carbon, pressure can be applied to the primary graphite sheet using a hot press or the like during graphitization. The pressure at this time can be, for example, 100kg / cm 2 Above, for example, it can be 200kg / cm 2 , for example, it can be 300kg / cm 2 The above, but not limited to.
[0065] According to one embodiment, the thickness of the graphite sheet may be 100 μm to 300 μm. According to another embodiment, the thickness of the graphite sheet may be 200 μm to 300 μm. When the thickness is within the above range, the handling property is excellent, but the present invention is not limited thereto.
[0066] According to one embodiment, the thermal diffusion coefficient of the graphite sheet can be 640 mm 2 / s or more. When it is within the above range, it can be more advantageous to be used as a heat dissipation mechanism in electronic equipment. For example, the thermal diffusion coefficient of a graphite sheet can be 650 mm 2 / s or more, for example, 670mm 2 / s or more, for example, 700mm 2 / s or more, but not limited to this.
[0067] According to one embodiment, the number of protrusions (bright spots) with a major diameter of 0.05 mm or more per unit area of 50 mm x 50 mm of the graphite sheet may be 5 or less. Within the above range, it can be more advantageous to use it as a heat dissipation mechanism used in electronic devices. For example, the number of bright spots generated per unit area of 50 mm x 50 mm of the graphite sheet may be 3 or less, or 2 or less, or 1 or less, or may not exist, but is not limited thereto.
[0068] Implementation
[0069] The present invention will be described in more detail below with reference to the following examples, but these are provided as preferred examples of the present invention and should not be construed in any way as limiting the present invention.
[0070] Example
[0071] Example 1
[0072] 100 g of pyromellitic dianhydride as a dianhydride monomer, 196 g of 4,4′-diaminodiphenyl ether as a diamine monomer, and 760 g of dimethylformamide as a solvent were mixed and reacted to prepare a polyamic acid solution having a viscosity of 200,000 cP.
[0073] Calcium hydrogen phosphate (average particle size (D 50 ):5μm)), 14g of acetic anhydride as a dehydrating agent, 2g of β-picoline as an imidizing agent and 10g of dimethylformamide as a solvent were used to prepare a precursor composition. At this time, the content of the sublimable inorganic filler used was 2,500ppm based on the weight of the polyimide film.
[0074] The precursor composition was cast on a SUS plate (100SA, Sandvik) using a doctor blade and dried at 130° C. for 8 minutes to produce a gel film. The gel film was separated from the SUS plate and then heat treated at 380° C. for 20 minutes to produce a polyimide film.
[0075] Example 2
[0076] A polyimide film was produced by the same method as in Example 1 except that the heat treatment temperature was changed from 380°C to 400°C.
[0077] Example 3
[0078] A polyimide film was produced by the same method as in Example 1 except that the heat treatment temperature was changed from 380°C to 420°C.
[0079] Comparative Example 1
[0080] A polyimide film was produced by the same method as in Example 1 except that the heat treatment temperature was changed from 380°C to 460°C.
[0081] Evaluation example
[0082] (1) 1 wt% loss thermal decomposition temperature (T d 1%) (unit: °C): The polyimide films produced in Examples and Comparative Examples were measured by thermogravimetric analysis using a thermogravimetric analyzer (TGA 5500, TA Corporation) at a heating rate of 10°C / min from room temperature (23°C) to 1,100°C.
[0083] (2) Color L*: The L* value was measured at room temperature using a colorimeter (Ultra scan pro, Hunter Lab).
[0084] (3) Thermal diffusivity (unit: mm 2 / s): The polyimide film manufactured in the embodiment and the comparative example is heated from room temperature to 1200°C at a heating rate of 1°C / min for carbonization, and then the polyimide film is graphitized at a heating rate of 1.5°C / min from 1200°C to 2200°C, at a heating rate of 0.4°C / min from 2200°C to 2500°C, and at a heating rate of 8.5°C / min from 2500°C to 2800°C, thereby manufacturing a graphite sheet.
[0085] The graphite sheet thus produced was cut into a circular shape having a diameter of 25.4 mm to produce a test piece, and the thermal diffusion coefficient of the test piece was measured by a laser flash method using a thermal diffusivity measuring device (LFA 467, Netsch).
[0086] (4) Bright spots (unit: number): The number of bright spots with a major diameter of 0.05 mm or more per unit area of 50 mm x 50 mm was measured.
[0087] [Table 1]
[0088]
[0089] As can be seen from Table 1 above, the high-thickness graphite sheets manufactured from the polyimide films of Examples 1 to 3 whose 1 wt% loss thermal decomposition temperature or L* value satisfies the range of the present invention have a high thermal diffusion coefficient and produce fewer bright spots, compared with the high-thickness graphite sheet manufactured from the polyimide film of Comparative Example 1 which does not meet the range of the present invention, and thus have excellent thermal conductivity and surface quality.
[0090] So far, the present invention has been understood with the embodiments as the center. A person skilled in the art of the present invention should be able to understand that the present invention can be implemented in a modified manner without departing from the essential characteristics of the present invention. Therefore, the disclosed embodiments should be considered from an illustrative point of view rather than a restrictive point of view. The scope of the present invention is shown in the claims rather than the above description, and all differences within the equivalent scope thereof will be interpreted as being included in the present invention.
[0091] Industrial Applicability
[0092] The present invention has the effect of providing a polyimide film for a graphite sheet which is excellent in surface quality and thermal conductivity and can ensure a high thickness, a method for producing the same, and a graphite sheet produced therefrom.
Claims
1. A polyimide film for a graphite sheet, having a thickness of 100 μm or more, a 1 wt% loss thermal decomposition temperature of 480° C. or less as measured by thermogravimetric analysis (TGA), and an L* value of 40 or more as measured by a colorimeter. Method for producing polyimide film for graphite sheet The following steps are involved: The polyamic acid solution is prepared by reacting a diamine monomer and a dianhydride monomer in a solvent; adding an imidizing agent, a dehydrating agent, and a sublimable inorganic filler to the polyamic acid solution to produce a precursor composition for a polyimide film; The precursor composition is coated on a support and dried to produce a gel film, wherein the drying of the precursor composition is performed at 30° C. to 200° C. for 15 seconds to 30 minutes; as well as The gel film is heat-treated to produce a polyimide film, wherein the heat treatment is performed at 250° C. to 420° C. for 30 seconds to 40 minutes. wherein the dianhydride monomer is selected from pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, oxydiphthalic anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride or a combination thereof, The diamine monomer is selected from 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane or a combination thereof. wherein the polyimide film contains a sublimable inorganic filler, The sublimable inorganic filler is selected from calcium hydrogen phosphate, barium sulfate, calcium carbonate or a combination thereof.
2. The polyimide film for a graphite sheet according to claim 1, wherein the average particle size D of the sublimable inorganic filler is 50 1μm to 10μm, The sublimable inorganic filler is contained in an amount of 0.15 to 0.25 parts by weight per 100 parts by weight of the polyimide film.
3. A graphite sheet, which is formed by carbonizing and graphitizing the polyimide film for graphite sheet according to claim 1 or 2, and has a thickness of 100 μm or more, wherein the thermal diffusion coefficient of the graphite sheet is 640 mm 2 / s or more.
4. A graphite sheet formed by carbonizing and graphitizing the polyimide film for a graphite sheet according to claim 1 or 2, having a thickness of 100 μm or more, wherein the number of protrusions, i.e., bright spots, having a major diameter of 0.05 mm or more per unit area of 50 mm x 50 mm of the graphite sheet is 5 or less.