A viscosity improving material for structural reinforcement sprayed polymer mortar
Through the combination of magnesium aluminum silicate, montmorillonite, diatomite and silica fume, the problem of balancing rheological properties and bonding properties in mortar viscosity adjustment is solved, and the construction performance and durability are improved to meet the dynamic load. the following requirements.
Patent Information
- Application Number
- CN202310533117.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-12
AI Technical Summary
It is difficult for existing viscosity adjustment materials to take into account both the rheological properties of the mortar before hardening and the bonding properties after hardening, and may even lead to conflicts. For example, cellulose ether materials improve the rheological properties but weaken the bonding strength.
Using a combination of magnesium aluminum silicate, montmorillonite, diatomite and silica fume, the viscosity of the mortar can be adjusted through specific ratios and particle size adjustments, which can not only improve the rheological properties of the mortar, but also improve its bonding performance.
It achieves excellent rheological construction performance before mortar hardening and high bonding strength performance after hardening, meets fatigue performance and durability performance under dynamic load, and avoids performance contradictions in the existing technology.
Smart Images

Figure BDA0004225079720000101 
Figure BDA0004225079720000111 
Figure BDA0004225079720000112
Abstract
Description
Technical Field
[0001] The invention relates to the field of highway bridge construction, in particular to a viscosity improving material for structure reinforcement sprayed polymer mortar. Background Art
[0002] Prestressed concrete highway bridges built in large numbers in the past 40 years generally face durability problems such as continuous deflection in the mid-span, cracking of the web and bottom plates, and corrosion of steel bars. They need to be reinforced. The method of increasing the cross-section is a commonly used reinforcement method. For example, the FRP rigid grid reinforcement system is a method of increasing the cross-section: this method uses high-performance continuous fibers such as carbon fiber and glass fiber to form an integral grid-like object in a resin with good corrosion resistance, and fixes it to the surface of the concrete component through anchor bolts, and then sprays polymer mortar to make it form a whole with the original concrete, thereby improving the bearing capacity and durability of the structure. The polymer mortar used in the system plays the role of protection, anti-corrosion, and bonding into a whole: under the protection of the polymer mortar, the impact resistance, fire resistance and durability of the reinforcement layer are improved. When performing anti-bending reinforcement, the stiffness and crack resistance of the reinforced component can also be improved.
[0003] Compared with ordinary cement mortar, the raw material composition of polymer repair mortar is different in that, in addition to cement and sand used in ordinary mortar, it also needs to be compounded with polymers and other types of performance adjustment additives, etc. 4-8 kinds of materials. This can greatly improve the anti-sagging construction performance / mechanical properties / anti-cracking performance / waterproof performance. Although the above additives are not added in large amounts (≤100kg per ton of mortar, i.e. ≤10%), they are indispensable for improving the performance of many aspects of mortar.
[0004] Among the many performance-adjusting additives, the most important category is viscosity-adjusting materials. Their main functions are as follows:
[0005] (1) Before the mortar hardens, improve the rheological properties of the mortar to facilitate top spraying construction.
[0006] (2) After the mortar hardens, improve the bonding properties of the mortar and ensure the bonding strength.
[0007] Existing viscosity regulating materials often cannot take into account or achieve the above two functions at the same time, and even produce contradictions. For example, cellulose ether materials commonly used in ordinary mortars are effective in improving the thixotropy of mortar before hardening, but will greatly affect the mechanical properties of mortar after hardening, weakening the interfacial bonding strength, resulting in a decrease in the mortar's flexural strength, compressive strength and bonding tensile strength. The greater the dosage, the greater the reduction.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The first purpose of the present invention is to provide a viscosity improving material for structural reinforcement sprayed polymer mortar. The viscosity improving material for structural reinforcement sprayed polymer mortar is used to adjust the viscosity of the mortar. It can improve the rheological properties of the mortar before the mortar hardens, and can also improve the bonding properties of the mortar after the mortar hardens.
[0010] The second purpose of the present invention is to provide a method for preparing the viscosity improving material for structural reinforcement sprayed polymer mortar. The method is simple and easy to operate, does not require a complicated preparation process, and the obtained viscosity improving material for structural reinforcement sprayed polymer mortar can take into account both the rheological properties and bonding properties of the mortar.
[0011] The third object of the present invention is to provide a mortar, which has excellent rheological construction performance before hardening and is easy to construct; and has good bonding strength performance after hardening, meeting the fatigue performance and durability performance under dynamic load.
[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0013] A viscosity improving material for structural reinforcement sprayed polymer mortar, comprising the following components in parts by weight:
[0014] 2-5 parts of magnesium aluminum silicate, 3-8 parts of montmorillonite, 8-12 parts of diatomaceous earth and 30-45 parts of silica fume.
[0015] Compared with the prior art, the viscosity regulating material overcomes the defect that the rheological property and the bonding property cannot be taken into consideration at the same time.
[0016] Preferably, the viscosity improving material for structural reinforcement sprayed polymer mortar comprises the following components in parts by weight:
[0017] 3-4 parts of magnesium aluminum silicate, 5-6 parts of montmorillonite, 9-11 parts of diatomaceous earth and 35-40 parts of silica fume.
[0018] Preferably, the particle size of the magnesium aluminum silicate is 250-300 meshes.
[0019] Preferably, the particle size of the montmorillonite is 180-230 meshes.
[0020] Preferably, the particle size of the diatomaceous earth is 300-400 meshes.
[0021] Preferably, the particle size of the silica fume is 800-1000 mesh.
[0022] The method for preparing the viscosity improving material for structural reinforcement sprayed polymer mortar comprises the following steps:
[0023] Mix all ingredients well.
[0024] The method is simple and easy to operate without complicated preparation process, and the obtained viscosity improving material for structure reinforcement sprayed polymer mortar can take into account both the rheological properties and the bonding properties of the mortar.
[0025] A mortar comprises the viscosity improving material for structural reinforcement sprayed polymer mortar obtained by preparing the viscosity improving material for structural reinforcement sprayed polymer mortar.
[0026] The mortar has excellent rheological construction performance before hardening and is easy to construct; and has good bonding strength performance after hardening, meeting the fatigue performance and durability performance under dynamic load.
[0027] Preferably, 30 to 100 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar are added to every 1000 parts of the mortar.
[0028] Preferably, the water retention rate of the mortar before hardening is 90-95%.
[0029] Preferably, the fluidity of the mortar before hardening is 190-210 mm.
[0030] Preferably, the initial shear yield stress of the mortar before hardening is 6.0-8.0 MPa.
[0031] Preferably, the 2h shear yield stress of the mortar before hardening is 26-32Mpa.
[0032] Preferably, the 28-day flexural strength of the mortar after hardening is 12.0-15.0 MPa.
[0033] Preferably, the 28-day compressive strength of the mortar after hardening is 55-60Mpa.
[0034] Preferably, the mortar has a 28-day bond tensile strength of 2.5-3.5 MPa after hardening.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The viscosity improving material for structure reinforcement sprayed polymer mortar provided by the present invention is a material for adjusting the viscosity of the mortar after magnesium aluminum silicate, montmorillonite, diatomaceous earth and silica fume are combined in a certain ratio. The material can improve the rheological properties of the mortar before the mortar hardens, and can also improve the bonding properties of the mortar after the mortar hardens. Compared with the prior art, the viscosity adjusting material overcomes the defect that both rheological properties and bonding properties cannot be taken into account at the same time.
[0037] (2) The method for preparing the viscosity improving material for structural reinforcement sprayed polymer mortar provided by the present invention is simple and easy to operate without requiring complicated preparation processes. The obtained viscosity improving material for structural reinforcement sprayed polymer mortar can take into account both the rheological properties and the bonding properties of the mortar.
[0038] (3) The mortar provided by the present invention has excellent rheological construction properties before hardening and is easy to construct; it has good bonding strength properties after hardening, meets the fatigue performance and durability performance under dynamic loads, and ensures the reinforcement effect. DETAILED DESCRIPTION
[0039] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] A viscosity improving material for structural reinforcement sprayed polymer mortar, comprising the following components in parts by weight:
[0041] 2-5 parts of magnesium aluminum silicate, 3-8 parts of montmorillonite, 8-12 parts of diatomaceous earth and 30-45 parts of silica fume.
[0042] In some specific embodiments, the magnesium aluminum silicate may be, for example, but not limited to, 2 parts, 3 parts, 4 parts or 5 parts.
[0043] In some specific embodiments, the montmorillonite may be, for example, but not limited to, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts or 8 parts.
[0044] In some specific embodiments, the diatomaceous earth may be, for example, but not limited to, 8, 9, 10, 11 or 12 parts.
[0045] In some specific embodiments, the silica fume may be, for example, but not limited to, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts or 45 parts.
[0046] The viscosity improving material for structural reinforcement sprayed polymer mortar is prepared by combining magnesium aluminum silicate, montmorillonite and silica fume in a certain ratio to adjust the viscosity of the mortar. It can improve the rheological properties of the mortar before the mortar hardens, and can also improve the bonding properties of the mortar after the mortar hardens. Compared with the prior art, the viscosity adjusting material overcomes the defect that the rheological properties and the bonding properties cannot be taken into account at the same time.
[0047] Before the mortar hardens, the rheological properties of the mortar are improved. That is, during the mortar spraying construction, it has good thixotropic properties. During the hardening stage of the mortar being shaped and leveled on the grid, it has good shape retention ability, so that it is easy to pump without blocking the pipe to ensure continuous construction, easy to atomize without lumps to ensure density without voids, easy to thixotropic and no sagging, and reduce material rebound loss.
[0048] After the mortar hardens, the bonding performance of the mortar is improved. That is, through the good interface bonding effect between the new mortar reinforcement layer and the old concrete reinforcement layer, high tensile bonding strength is achieved, ensuring reliable connection between the mortar layer and the reinforced structural layer, achieving deformation coordination, and meeting fatigue performance and durability performance under dynamic loads.
[0049] The magnesium aluminum silicate used in the present invention includes but is not limited to powder materials.
[0050] The montmorillonite used in the present invention includes but is not limited to powder materials.
[0051] The silica fume used in the present invention includes but is not limited to powder materials.
[0052] Preferably, the viscosity improving material for structural reinforcement sprayed polymer mortar comprises the following components in parts by weight:
[0053] 3-4 parts of magnesium aluminum silicate, 5-6 parts of montmorillonite, 9-11 parts of diatomaceous earth and 35-40 parts of silica fume.
[0054] Preferably, the particle size of the magnesium aluminum silicate is 250-300 meshes.
[0055] In some specific embodiments, the particle size of the magnesium aluminum silicate may be, for example, but not limited to, 250 mesh, 260 mesh, 270 mesh, 280 mesh, 290 mesh or 300 mesh.
[0056] Preferably, the particle size of the montmorillonite is 180-230 meshes.
[0057] In some specific embodiments, the particle size of the montmorillonite may be, for example, but not limited to, 180 mesh, 190 mesh, 200 mesh, 210 mesh, 220 mesh or 230 mesh.
[0058] Preferably, the particle size of the diatomaceous earth is 300-400 meshes.
[0059] In some specific embodiments, the particle size of the diatomaceous earth may be, for example, but not limited to, 300 mesh, 320 mesh, 340 mesh, 360 mesh, 380 mesh or 400 mesh.
[0060] Preferably, the particle size of the silica fume is 800-1000 mesh.
[0061] In some specific embodiments, the particle size of the silica fume may be, for example, but not limited to, 800 mesh, 850 mesh, 900 mesh, 950 mesh or 1000 mesh.
[0062] The method for preparing the viscosity improving material for structural reinforcement sprayed polymer mortar comprises the following steps:
[0063] Mix all ingredients well.
[0064] The method for preparing the viscosity improving material for structural reinforcement sprayed polymer mortar is simple, easy to operate, and does not require complicated preparation processes. The obtained viscosity improving material for structural reinforcement sprayed polymer mortar can take into account both the rheological properties and the bonding properties of the mortar.
[0065] A mortar comprises the viscosity improving material for structural reinforcement sprayed polymer mortar obtained by preparing the viscosity improving material for structural reinforcement sprayed polymer mortar.
[0066] The mortar has excellent rheological construction performance before hardening and is easy to construct; and has good bonding strength performance after hardening, meeting the fatigue performance and durability performance under dynamic load.
[0067] Preferably, 30 to 100 parts (eg, 30, 40, 50, 60, 70, 80, 90 or 100 parts) of the viscosity improving material for structural reinforcement sprayed polymer mortar are added to every 1000 parts of the mortar.
[0068] Preferably, the mortar comprises the following components in parts by mass:
[0069] The structure reinforcement spray polymer mortar comprises 30 to 100 parts of viscosity improving material, 500 to 670 parts of sand and 300 to 400 parts of cement.
[0070] Preferably, the water retention rate of the mortar before hardening is 90-95%.
[0071] Preferably, the fluidity of the mortar before hardening is 190-210 mm.
[0072] Preferably, the initial shear yield stress of the mortar before hardening is 6.0-8.0 MPa.
[0073] Preferably, the 2h shear yield stress of the mortar before hardening is 26-32Mpa.
[0074] Preferably, the 28-day flexural strength of the mortar after hardening is 12.0-15.0 MPa.
[0075] Preferably, the 28-day compressive strength of the mortar after hardening is 55-60Mpa.
[0076] Preferably, the mortar has a 28-day bond tensile strength of 2.5-3.5 MPa after hardening.
[0077] The embodiments of the present invention will be described in detail below with reference to specific examples and comparative examples.
[0078] Example 1
[0079] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this embodiment includes the following components in parts by weight:
[0080] 5 parts of magnesium aluminum silicate, 8 parts of montmorillonite, 12 parts of diatomaceous earth and 45 parts of silica fume.
[0081] Example 2
[0082] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this embodiment includes the following components in parts by weight:
[0083] 2 parts of magnesium aluminum silicate, 3 parts of montmorillonite, 8 parts of diatomaceous earth and 30 parts of silica fume.
[0084] Example 3
[0085] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this embodiment includes the following components in parts by weight:
[0086] 4 parts of magnesium aluminum silicate, 5 parts of montmorillonite, 11 parts of diatomaceous earth and 35 parts of silica fume.
[0087] Example 4
[0088] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this embodiment includes the following components in parts by weight:
[0089] 3 parts of magnesium aluminum silicate, 6 parts of montmorillonite, 9 parts of diatomaceous earth and 40 parts of silica fume.
[0090] Example 5
[0091] The mortar provided in this embodiment includes the following components by weight:
[0092] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar of Example 1.
[0093] Example 6
[0094] The mortar provided in this embodiment includes the following components by weight:
[0095] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar of Example 2.
[0096] Example 7
[0097] The mortar provided in this embodiment includes the following components by weight:
[0098] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar of Example 3.
[0099] Example 8
[0100] The mortar provided in this embodiment includes the following components by weight:
[0101] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar of Example 4.
[0102] Comparative Example 1
[0103] The mortar provided in this comparative example includes the following components by weight:
[0104] PO52.5 cement 340 parts, 30-80 mesh sand 630 parts, water 140 parts and cellulose ether 0.2 parts.
[0105] Comparative Example 2
[0106] The mortar provided in this comparative example includes the following components by weight:
[0107] PO52.5 cement 340 parts, 30-80 mesh sand 630 parts and water 140 parts.
[0108] Comparative Example 3
[0109] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this comparative example comprises the following components in parts by weight:
[0110] 6 parts of magnesium aluminum silicate, 9 parts of montmorillonite, 17 parts of diatomaceous earth and 25 parts of silica fume.
[0111] The mortar provided in this comparative example includes the following components by weight:
[0112] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the above-mentioned viscosity improving material for structural reinforcement sprayed polymer mortar.
[0113] Comparative Example 4
[0114] The viscosity improving material for structural reinforcement sprayed polymer mortar provided in this comparative example comprises the following components in parts by weight:
[0115] 23 parts of magnesium aluminum silicate, 26 parts of montmorillonite and 9 parts of diatomaceous earth.
[0116] The mortar provided in this comparative example includes the following components by weight:
[0117] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 30 parts of the above-mentioned viscosity improving material for structural reinforcement sprayed polymer mortar.
[0118] Comparative Example 5
[0119] The mortar provided in this comparative example includes the following components by weight:
[0120] 340 parts of PO52.5 cement, 630 parts of 30-80 mesh sand, 140 parts of water and 120 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar of Example 4.
[0121] Experimental example
[0122] The performance of the mortars of the embodiments and comparative examples was tested, and the results are shown in Tables 1 and 2.
[0123] Table 1 Rheological construction properties of mortar before hardening
[0124]
[0125]
[0126] Table 2 Bond strength properties of mortar after hardening
[0127]
[0128] From the comparative data of Tables 1 and 2, it can be seen that after using the viscosity improving material for structural reinforcement sprayed polymer mortar of the present invention, the rheological construction performance of the mortar before hardening and the bonding strength performance of the mortar after hardening can be significantly improved;
[0129] Compared with the traditional cellulose ether, after using the material of the present invention, the rheological construction performance of the mortar before hardening can be kept close to that of the traditional cellulose ether, and the pumping performance is better than that of the cellulose ether. At the same time, in terms of the bonding strength performance of the mortar after hardening, it is significantly better than that of the cellulose ether, avoiding the defect of strength attenuation caused by the use of cellulose ether.
[0130] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A viscosity improving material for structural reinforcement sprayed polymer mortar, It is characterized in that By weight, it is composed of the following components: 2-5 parts of magnesium aluminum silicate, 3-8 parts of montmorillonite, 8-12 parts of diatomaceous earth and 30-45 parts of silica fume.
2. The viscosity improving material for structural reinforcement sprayed polymer mortar according to claim 1, It is characterized in that By weight, it is composed of the following components: 3-4 parts of magnesium aluminum silicate, 5-6 parts of montmorillonite, 9-11 parts of diatomaceous earth and 35-40 parts of silica fume.
3. The viscosity improving material for structural reinforcement sprayed polymer mortar according to claim 1 or 2, It is characterized in that The particle size of the magnesium aluminum silicate is 250-300 meshes.
4. The viscosity improving material for structural reinforcement sprayed polymer mortar according to claim 1 or 2, It is characterized in that The particle size of the montmorillonite is 180-230 meshes.
5. The viscosity improving material for structural reinforcement sprayed polymer mortar according to claim 1 or 2, It is characterized in that The particle size of the diatomaceous earth is 300-400 meshes.
6. The viscosity improving material for structural reinforcement sprayed polymer mortar according to claim 1 or 2, It is characterized in that The particle size of the silica fume is 800-1000 meshes.
7. A method for preparing a viscosity improving material for structural reinforcement sprayed polymer mortar according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Mix all ingredients well.
8. A mortar, It is characterized in that The viscosity improving material for structural reinforcement sprayed polymer mortar comprises the material described in any one of claims 1 to 6.
9. The mortar according to claim 8, It is characterized in that 30 to 100 parts of the viscosity improving material for structural reinforcement sprayed polymer mortar are added to every 1000 parts of the mortar.
10. The mortar according to claim 8, It is characterized in that The water retention rate of the mortar before hardening is 90-95%.
11. The mortar according to claim 8, It is characterized in that The fluidity of the mortar before hardening is 190-210 mm.
12. The mortar according to claim 8, It is characterized in that The initial shear yield stress of the mortar before hardening is 6.0-8.0 MPa.
13. The mortar according to claim 8, It is characterized in that The 2h shear yield stress of the mortar before hardening is 26-32MPa.
14. The mortar according to claim 8, It is characterized in that The 28-day flexural strength of the mortar after hardening is 12.0-15.0 MPa.
15. The mortar according to claim 8, It is characterized in that The 28-day compressive strength of the mortar after hardening is 55-60 MPa.
16. The mortar according to claim 8, It is characterized in that The mortar has a 28-day bond tensile strength of 2.5-3.5 MPa after hardening.
Citation Information
Patent Citations
Dangerous outer wall heat insulation board grouting and reinforcing mortar