A method for synthesizing polyalphaolefin lubricant base oil

By using AlCl3 and silane or oxysilane catalyst system in the synthesis of poly-alpha-olefin lubricating oil, the problems of local exotherm and excessive viscosity caused by AlCl3 are solved, and mild reaction and controllable product performance are achieved.

CN116574204BActive Publication Date: 2024-10-22SINOCHEM QUANZHOU PETROCHEM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310509046.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-10-22
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

In the process of synthesizing poly-alpha-olefin lubricating oil, the AlCl3 catalyst causes a large local heat release, the product viscosity is too high, and the production process is difficult to stably control.

Method used

A catalyst system using AlCl3 and silane or oxysilane as an electron donor is used to adjust the acidity of AlCl3, making the reaction mild and controlling the viscosity and pour point of the product.

Benefits of technology

The mildness and stability of the reaction process are achieved, lower viscosity and pour point are obtained, as well as higher product yield and viscosity index.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a method for synthesizing a poly-alpha-olefin lubricant base oil. When a catalyst composed of AlCl3 and a silane electron donor is used to synthesize poly-alpha-olefin synthetic oil, the method has the advantages of high activity, mild reaction process, adjustable product viscosity, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lubricant base oil preparation, and in particular relates to a method for synthesizing poly-alpha-olefin lubricant base oil. Background Art

[0002] In recent years, as the speed of lubricant upgrading has become faster and faster, the market demand for high-end lubricant products has driven the rapid growth of demand for polyalphaolefin (PAO) base oil. Compared with mineral oil, PAO synthetic oil has better antioxidant stability and viscosity-temperature performance, high viscosity index, low pour point, good sensitivity to additives, and can be mixed with mineral oil in any proportion. Due to its excellent physical and chemical properties, PAO has been widely used in aerospace, military industry, high-end automobiles and other fields.

[0003] At present, the global PAO base oil production capacity is relatively concentrated, among which the top three producers INEOS, ExxonMobil and Chevron account for more than 90% of the global production capacity. The catalysts used to synthesize PAO mainly include AlCl3, BF3, metallocene and ionic liquid catalysts. Due to the low price and mild reaction conditions of AlCl3 catalyst, it is still the mainstream PAO catalyst in China.

[0004] Chevron's patent US8115040B2 discloses a method for synthesizing PAO using AlCl3 as a catalyst, in which a small amount of HCl is added as a promoter, and the product has a pour point of less than -50°C and a viscosity index of at least 134. Chevron's patent US8178739B2 discloses a method for synthesizing PAO using AlCl3 as a catalyst. The patent adjusts the oligomerization step to produce a base oil with a kinematic viscosity of 20 to 90. East China University of Science and Technology (CN201310260208.2) uses a mixture of AlCl3 and TiCl4 as a catalyst, which can be used in the industrial production of coal wax cracking olefins to synthesize polyalphaolefin lubricant base oil. CN101977879A and CN105925340A disclose a method for preparing oligomeric polyalphaolefins, comprising oligomerizing low molecular weight PAO oligomers under oligomerization conditions in the presence of a Lewis acid catalyst such as promoted AlCl3 or BF3. The low molecular weight PAO oligomer used as feed or feed component of the method is a light olefinic byproduct fraction, which contains dimers and light fractions from the metallocene-catalyzed PAO oligomerization process, with a molecular weight of 150 to 600 and a terminal olefin (vinylidene) content of at least 25%. US12261388 and US12538746 use AlCl3 as a catalyst to obtain a series of base oil products with a viscosity index of up to 145 and a pour point of -54°C. AlCl3 is also used in ionic liquid catalyst systems. US8222471B2 uses olefins with boiling points lower than 82°C to obtain a kinematic viscosity greater than 1100 mm at 40°C. 2 / s lubricating oil base oil; US12763866 uses AlCl3 and 1-butylpyridinium chloride to prepare an ionic liquid catalyst, and prepares a lubricating oil synthetic oil with a viscosity index not less than 134 but a pour point not higher than -28 ℃ by alkylating oligoolefins.

[0005] According to a large number of disclosed patents or reports, due to the strong acidity of AlCl3, there is large local heat release during the synthesis of PAO, the product viscosity is too high, and the production process is difficult to stably control. Summary of the invention

[0006] In order to solve the above technical problems, the present invention discloses a method for synthesizing lubricating oil base oil of poly-alpha-olefin, and the present invention relates to a catalyst system for synthesizing poly-alpha-olefin, comprising AlCl3 and silane electron donor. The present invention claims that a catalyst composed of AlCl3 and silane electron donor has the advantages of high activity, mild reaction process, adjustable product viscosity, etc. when used for synthesizing poly-alpha-olefin synthetic oil.

[0007] The present invention claims a method for synthesizing a lubricating oil base oil of poly-alpha-olefins, wherein the catalyst used in the method is composed of the following two parts:

[0008] (1) Main catalyst: AlCl3;

[0009] (2) Electron donor: one of diphenyldimethoxysilane, phenyltriethoxysilane, cyclohexylmethyldimethoxysilane, dichloro(methyl)phenylsilane, dichlorodiphenylsilane, triphenylchlorosilane, trimethylchlorosilane

[0010] Further, the molar ratio of the electron donor to AlCl3 is 0.001~0.1:1;

[0011] Further, the raw materials used for the poly-α-olefin synthesis reaction are 1-octene, 1-decene, 1-dodecene, and a mixture of any two or three of the above α-olefins;

[0012] Further, in the poly-alpha-olefin synthesis reaction, the mass ratio of catalyst to raw material is 0.001~0.1:1;

[0013] Furthermore, the poly-α-olefin synthesis reaction is mainly carried out in an inert solvent, and the inert solvent, AlCl3, and electron donor are injected into the reactor in sequence, and finally the reaction raw materials are added at a temperature of 30-150 o C, react for 0.1~10h under stirring;

[0014] Furthermore, the solvent is one of hexane, cyclohexane, methylcyclohexane and 1,2-dichloroethane.

[0015] Furthermore, the method for synthesizing a lubricating oil base oil of poly-alpha-olefin comprises the following steps:

[0016] 1) Take out the three-necked flask and rotor that have been dried in advance and weigh them. The three necks are connected to a thermocouple, a condenser, and a turn-over stopper respectively; weigh the required raw materials, solvents, and catalysts in the glove box; turn on the vacuum pump, turn the double-row tube to the vacuum position, and evacuate the three-necked flask to room temperature; turn on the nitrogen, slowly adjust the double-row tube to the nitrogen position, and be sure to prevent backflow; switch the vacuum-nitrogen environment three times, and finally keep the device in a nitrogen environment, and turn off the vacuum pump; turn on stirring, turn on condensing water, turn on the heating device, and inject an inert solvent into the turn-over stopper with a syringe; heat up to 50 °C, quickly remove the sealing stopper, pour in AlCl3 powder, and then inject the electron donor; heat up to a certain temperature, inject α-olefin with a syringe, turn the three-way valve above the condenser to the three-way, adjust the nitrogen, react for a while, and weigh the syringe and weighing bottle.

[0017] 2) Add ultrapure water to the prepared sample and stir it magnetically for several minutes, then let it stand in a separatory funnel to separate the liquid, collect the oil phase and continue washing with water for three times. Add anhydrous sodium sulfate and let it stand for several hours; remove the sodium sulfate solid by vacuum filtration; distill the obtained oil under reduced pressure until no droplets appear on the wall of the condenser tube. Weigh the obtained product, test the viscosity and pour point, and calculate the yield.

[0018] The present invention adopts silane electron donor for the first time to adjust the acidity of AlCl3, so that the heat release in the process of synthesizing PAO is small, mild and easy to control.

[0019] The present invention uses a silane electron donor to adjust the acidity of the AlCl3 catalyst, and the prepared catalyst system has the following advantages: (1) the acidity of AlCl3 can be appropriately adjusted to make the reaction mild and easy to control; (2) the viscosity and pour point of the PAO product can be controlled by adjusting the amount of the electron donor added, and a PAO product with low viscosity and low pour point can be obtained; (3) the silane electron donor is inexpensive and easy to obtain. DETAILED DESCRIPTION

[0020] In order to make the above features and advantages of the present invention more clearly understood, the following embodiments are given for detailed description. The methods of the present invention are all conventional methods in the art unless otherwise specified.

[0021] Embodiment 1:

[0022] The poly-α-olefin synthesis experiment was carried out in a three-necked flask. Take out the three-necked flask and rotor that had been dried in advance and weigh them. The three flasks were connected to a thermocouple, a condenser, and a turn-over stopper respectively; weigh the required raw materials, solvents, and catalysts in the glove box; turn on the vacuum pump, turn the double-row tube to the vacuum position, and evacuate the three-necked flask to room temperature; turn on the nitrogen, slowly adjust the double-row tube to the nitrogen position, and be sure to prevent back suction; switch the vacuum-nitrogen environment three times, and finally keep the device in a nitrogen environment, turn off the vacuum pump; turn on the stirring, turn on the condenser, turn on the heating setting to 70 °C, and inject 40 ml of cyclohexane into the turn-over stopper with a syringe; heat up to 50 °C, quickly remove the sealing stopper, pour in 3 g of AlCl3 powder main catalyst, and inject dichlorodiphenylsilane (0.2 g) electron donor diluted with cyclohexane in advance with a syringe; heat up to 70 °C, inject 80 ml of 1-decene with a syringe, turn the three-way valve above the condenser to the three-way, adjust the nitrogen, react for 2 h, and weigh the syringe and weighing bottle. Ultrapure water was added to the prepared sample and magnetically stirred for several minutes, then the sample was allowed to stand in a separatory funnel for separation, and the oil phase was collected and washed with water three times. 1 g of anhydrous sodium sulfate was added and allowed to stand for several hours; sodium sulfate solids were removed by vacuum filtration; the obtained oil was heated at 130 °C. o The vacuum distillation was carried out at a temperature of 100 °C until no droplets appeared on the wall of the condenser tube. The obtained product was weighed, the viscosity and pour point were tested, and the yield was calculated. The data results are shown in Table 1.

[0023] Embodiment 2:

[0024] The process is basically the same as Example 1, except that the electron donor is replaced with diphenyldimethoxysilane. The data results are shown in Table 1.

[0025] Embodiment 3:

[0026] The process is basically the same as Example 1, except that the electron donor is replaced with cyclohexylmethyldimethoxysilane. The data results are shown in Table 1.

[0027] Embodiment 4:

[0028] The process is basically the same as Example 1, except that the solvent is changed to methylcyclohexane. The data results are shown in Table 1.

[0029] Embodiment 5:

[0030] The same as Example 4, except that the reaction temperature was changed to 110 o C, the data results are shown in Table 1.

[0031] Comparative Example 1:

[0032] The process is basically the same as Example 1, except that the catalyst is only AlCl3 and no electron donor is added. The data results are shown in Table 1.

[0033] Table 1

[0034]

[0035] As shown in Table 1, silane or oxysilane is used in combination with AlCl3 as a PAO synthesis catalyst, and the PAO obtained by the system of using AlCl3 catalyst alone has a higher product yield, a lower viscosity and a pour point, and a higher viscosity index. This area usually uses a single AlCl3 catalyst or AlCl3 and an auxiliary agent such as alcohol or water to adjust the activity and electrical properties of the AlCl3 catalyst, but the above scheme still has problems such as violent reaction, severe overheating, and difficulty in controlling the reaction process. Due to the violent reaction, uneven distribution of raw materials, high degree of polymerization of raw materials, high viscosity of products and high pour point, etc. can be caused. The silane or oxysilane used in the present invention can form coordination with AlCl3, and its electron-donating performance can weaken the acidity of AlCl3, so that it releases acidity gently, resulting in a gentle reaction process, uniform products, and a high product yield, viscosity and pour point are all lower.

[0036] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for synthesizing a poly-alpha-olefin lubricant base oil, characterized in that: The catalyst used in this method consists of the following two parts composition: (1) Main catalyst: AlCl3; (2) Electron donor: one of diphenyldimethoxysilane, phenyltriethoxysilane, cyclohexylmethyldimethoxysilane, dichloro(methyl)phenylsilane, dichlorodiphenylsilane, triphenylchlorosilane, and trimethylchlorosilane; The molar ratio of electron donor to AlCl3 is 0.001~0.1:

1.

2. The method for synthesizing poly-alpha-olefin lubricant base oil according to claim 1, characterized in that: The raw materials used for the poly-alpha-olefin synthesis reaction are one or more of 1-octene, 1-decene and 1-dodecene.

3. The method for synthesizing poly-alpha-olefin lubricant base oil according to claim 2, characterized in that: In the poly-α-olefin synthesis reaction, the mass ratio of catalyst to raw material is 0.001~0.1:

1.

4. The method for synthesizing poly-alpha-olefin lubricant base oil according to claim 1, characterized in that: The poly-α-olefin synthesis reaction is carried out in an inert solvent. The inert solvent, AlCl3, and electron donor are injected into the reactor in sequence, and finally the reaction raw materials are added at a temperature of 30-150 o C, react for 0.1~10h under stirring.

5. The method for synthesizing poly-alpha-olefin lubricant base oil according to claim 4, characterized in that: The solvent is one of hexane, cyclohexane, methylcyclohexane and 1,2-dichloroethane.