A water-based environmentally friendly wear-resistant epoxy floor paint and preparation method thereof
By wrapping MoS2 nanoribbons on carbon nanotubes and adding a specific curing agent, the problem of reduced wear resistance of epoxy floor paint in high temperature and humid environments is solved, achieving higher wear resistance and adhesion, and prolonging the service life.
Patent Information
- Application Number
- CN202310581541.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The wear resistance of existing epoxy floor paints decreases in high temperature and humid environments, and the adhesion is insufficient, resulting in accelerated wear.
Water-based environmentally friendly and wear-resistant epoxy floor paint is used, by wrapping MoS2 nanoribbons on carbon nanotubes, and adding thiourea, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex, To improve the self-lubricating performance and self-healing ability of the paint film.
It significantly improves the wear resistance and adhesion of epoxy floor paint and extends its service life, especially in high temperature and humid environments.
Smart Images

Figure SMS_3 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of floor coatings, and more specifically, to a water-based, environmentally friendly, wear-resistant epoxy floor coating and a preparation method thereof. Background Art
[0002] Floor coatings are mainly divided into epoxy floor coatings, polyurethane floor coatings, vinyl floor coatings and acrylic floor coatings. They are a type of building floor decoration material mainly used in industrial plants, warehouses, parking lots, shopping malls, stadiums, schools, hospitals and offices.
[0003] Among them, epoxy floor paint refers to a polymer coating that uses epoxy resin as the main film-forming substrate and is cross-linked into a network structure through a curing agent. Epoxy floor paint is also widely used in the field of adhesives and composite materials because of its excellent adhesion, thermal stability, chemical resistance, insulation and mechanical strength.
[0004] However, although epoxy floor paint has excellent adhesion, wear and tear will still occur in areas where workers move more frequently during actual work. Therefore, there is an urgent need for an epoxy floor paint with better wear resistance. Summary of the invention
[0005] In order to further improve the wear resistance of epoxy floor paint, the present application provides a water-based environmentally friendly wear-resistant epoxy floor paint and a preparation method thereof.
[0006] The present application provides a water-based, environmentally friendly, wear-resistant epoxy floor paint that adopts the following technical solutions:
[0007] In the first aspect, the present application provides a water-based environmentally friendly wear-resistant epoxy floor paint, which adopts the following technical solution:
[0008] A water-based, environmentally friendly, wear-resistant epoxy floor paint, which consists of a component A and a component B, wherein the mass ratio of the component A to the component B is (2-4):1;
[0009] The component A comprises the following raw materials in parts by weight: 90-110 parts of waterborne epoxy resin, 20-30 parts of carbon nanotube-wrapped MoO3-MoS2 nanobelts, 1-5 parts of dispersant, 1-5 parts of defoamer and 1-5 parts of film-forming aid;
[0010] The B component includes the following raw materials in parts by weight: 30-50 parts of deionized water and 20-40 parts of epoxy resin curing agent.
[0011] MoS2 belongs to the hexagonal crystal system. Its crystal structure is similar to that of graphite, both of which are close-packed hexagonal structures with layered structures. Mo-S has many facets and a large specific surface area. Moreover, the layers of MoS2 are bonded to each other by weak van der Waals forces and are bonded within the layers by covalent bonds. The layers are easy to slip along the close-packed structure and are easily peeled off. It has good anisotropy and a low friction coefficient, which makes the epoxy floor paint containing MoS2 have excellent wear resistance.
[0012] However, when epoxy floor paint is used in a high temperature and humid environment, the surface of MoS2 is easily oxidized, which leads to a sharp decrease in the tribological properties of MoS2, and then the wear resistance of the epoxy floor paint containing MoS2 is also significantly decreased.
[0013] Carbon nanotube-coated metal oxide has a graphene-like structure and has excellent self-lubricating properties. Similarly, carbon nanotube-coated MoO3-MoS2 nanobelts not only have self-lubricating properties, but can also effectively protect MoS2, thereby effectively reducing the possibility of further oxidation of MoS2 and further improving the wear resistance of epoxy floor paint.
[0014] Preferably, the method for preparing the carbon nanotube-wrapped MoO3-MoS2 nanobelt comprises the following steps:
[0015] 1) drying the MoO3-MoS2 precursor nanobelt and adding it to distilled water for dispersion, and then adding polydiallyldimethylammonium chloride for further dispersion to obtain a MoO3-MoS2 precursor nanobelt preform;
[0016] 2) adding a MoO3-MoS2 precursor nanobelt preparation dropwise into the carbon nanotube dispersion, followed by filtration and drying, then removing the dried membrane from the filter membrane, and annealing the membrane in a protective gas environment to obtain carbon nanotube-wrapped MoO3-MoS2 nanobelts.
[0017] In 1), after the MoO3-MoS2 precursor nanobelts are dispersed in water, the cationic electrolyte polydiallyldimethylammonium chloride is added to continue dispersing. Therefore, the surface of MoO3 will be positively charged, while the surface of the carbon nanotube dispersion will be negatively charged. After the two are mixed, the positive and negative charges attract each other. Compared with simple mechanical mixing, this method can cause the carbon nanotubes to be tightly coated on the surface of the MoO3-MoS2 precursor nanobelt preparation, further improving the wear resistance of the epoxy floor paint.
[0018] Preferably, the mass ratio of the MoO3-MoS2 precursor nanobelt, polydiallyldimethylammonium chloride and carbon nanotube dispersion is (0.1-0.2):(4-8):(30-40).
[0019] When the MoO3-MoS2 precursor nanobelts, polydiallyldimethylammonium chloride and carbon nanotube dispersion are in the above mass ratio, the carbon nanotubes can be more tightly coated on the surface of the MoO3-MoS2 precursor nanobelt preparation, thereby further improving the wear resistance of the epoxy floor paint.
[0020] Preferably, the method for preparing the MoO3-MoS2 precursor nanobelt comprises the following steps:
[0021] A) heating MoS2 powder to 400-600°C in an oxygen environment, and then grinding the product to obtain nano-scale MoO3-MoS2 powder;
[0022] B) Add nano-sized MoO3-MoS2 powder to deionized water for dilution and stirring, and then heat to 150-200°C for hydrothermal reaction. Then cool naturally, wash and freeze-dry to obtain MoO3-MoS2 precursor nanobelts.
[0023] When MoS2 powder is heated to 400-600℃ in an oxygen environment, MoO3 will form on the surface of the MoS2 powder. After grinding the product, the prepared powder will have both MoO3 and MoS2, which enables the powder to form nanobelts and effectively connect with carbon nanotubes.
[0024] Preferably, the particle size of the MoS2 powder is between 50-80 μm, and the particle size of the nano-scale MoO3-MoS2 powder is between 500-800 nm.
[0025] When the particle size of MoS2 powder is between 50-80μm and the particle size of nano-scale MoO3-MoS2 powder is between 500-800nm, the contents of MoO3 and MoS2 in the nano-scale MoO3-MoS2 powder are uniform, and the effect of improving the wear resistance of epoxy floor paint is more prominent.
[0026] Preferably, the film-forming aid is propylene glycol methyl ether, and the epoxy resin curing agent includes thiourea and diethylenetriamine.
[0027] When propylene glycol methyl ether is used as a film-forming aid, although the surface drying time of the epoxy floor paint is extremely short, the interior of the epoxy floor paint is not completely cured, resulting in relatively poor adhesion of the epoxy floor paint, and then resulting in relatively poor wear resistance of the epoxy floor paint.
[0028] Thiourea can promote the activity of various amine-cured epoxy resins. The reason is that the nucleophilicity of the sulfur atom in thiourea is much greater than the nucleophilicity of the nitrogen atom in various amines. Compared with amines, thiourea can react with epoxy groups at a lower temperature or at a higher speed. This reaction is an exothermic reaction, which increases the temperature of the epoxy mixture near the thiourea, thereby promoting the reaction of itself and various amines with epoxy groups, and then promoting the complete curing of the interior of the epoxy floor paint, effectively improving the adhesion of the epoxy floor paint, and indirectly improving the wear resistance of the epoxy floor paint.
[0029] Preferably, the epoxy resin curing agent further comprises 4,4'-dithiodiphenylamine and chitosan-copper chloride complex.
[0030] 4,4'-Disulfide diphenylamine is an amine curing agent containing a disulfide bond. The disulfide bond itself has low bond energy and is easy to break. Therefore, the disulfide bond can be easily broken and reorganized, thereby achieving a reversible dynamic exchange reaction, thereby enabling the epoxy floor paint to have a self-healing function.
[0031] In the chitosan-copper chloride complex, copper chloride has a self-repair promoting effect, while chitosan contains rich amino, acetyl and hydroxyl groups, which will interact with each other and form a diverse hydrogen bond network, thereby further improving the wear resistance of epoxy floor paint.
[0032] Preferably, the mass ratio of thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex is (0.3-0.6):1:(1.0-1.6):(0.2-0.4).
[0033] By adopting the above technical solution, when thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex are used in the above mass ratio, the epoxy floor paint has better self-healing performance and wear resistance.
[0034] In the second aspect, the present application provides a method for preparing a water-based, environmentally friendly, wear-resistant epoxy floor paint, using the following technical solution:
[0035] A method for preparing a water-based, environmentally friendly, wear-resistant epoxy floor paint comprises the following steps:
[0036] S1, mixing and stirring a water-based epoxy resin, a carbon nanotube-wrapped MoO3-MoS2 nanobelt, a dispersant, a defoaming agent and a film-forming aid to obtain a component A;
[0037] S2, mixing deionized water and epoxy resin curing agent to obtain component B;
[0038] S3, mixing component A and component B to obtain a water-based, environmentally friendly, wear-resistant epoxy floor paint.
[0039] In summary, this application has the following beneficial effects:
[0040] 1. MoS2 belongs to the hexagonal crystal system. Its crystal structure is similar to that of graphite. Both are close-packed hexagonal structures with layered structures. Mo-S has many facets and a large specific surface area. The layers of MoS2 are bonded to each other by weak van der Waals forces and are bonded within the layers by covalent bonds. The layers are easy to slip along the close packing and are easy to peel off. It has good anisotropy and a low friction coefficient, which makes the epoxy floor paint containing MoS2 have excellent wear resistance.
[0041] 2. Carbon nanotubes coated with metal oxides have a graphene-like structure, which itself has excellent self-lubricating properties. Similarly, carbon nanotubes wrapped in MoO3-MoS2 nanobelts not only have self-lubricating properties, but can also effectively protect MoS2, thereby effectively reducing the possibility of further oxidation of MoS2 and further improving the wear resistance of epoxy floor paint.
[0042] 3. After the MoO3-MoS2 precursor nanobelts are dispersed in water, the cationic electrolyte polydiallyldimethylammonium chloride is added to continue dispersing. Therefore, the surface of MoO3 will be positively charged, while the surface of the carbon nanotube dispersion will be negatively charged. After the two are mixed, the positive and negative charges attract each other. Compared with simple mechanical mixing, this method can cause the carbon nanotubes to be tightly coated on the surface of the MoO3-MoS2 precursor nanobelt preparation, further improving the wear resistance of the epoxy floor paint.
[0043] 4. Thiourea can promote the activity of various amine-cured epoxy resins. The reason is that the nucleophilicity of sulfur atoms in thiourea is much greater than the nucleophilicity of nitrogen atoms in various amines. Compared with amines, thiourea can react with epoxy groups at lower temperatures or at higher speeds. This reaction is an exothermic reaction, which increases the temperature of the epoxy mixture near thiourea, thereby promoting the reaction of itself and various amines with epoxy groups, and then promoting the complete curing of the interior of the epoxy floor paint, effectively improving the adhesion of the epoxy floor paint, and indirectly improving the wear resistance of the epoxy floor paint.
[0044] 5. 4,4'-disulfide diphenylamine is an amine curing agent containing a disulfide bond. The disulfide bond itself has low bond energy and is easy to break. Therefore, the disulfide bond can be easily broken and reorganized, thereby realizing a reversible dynamic exchange reaction, thereby enabling the epoxy floor paint to have a self-healing function.
[0045] In the chitosan-copper chloride complex, copper chloride has a self-repair promoting effect, while chitosan contains rich amino, acetyl and hydroxyl groups, which will interact with each other and form a diverse hydrogen bond network, thereby further improving the wear resistance of epoxy floor paint. DETAILED DESCRIPTION
[0046] The present application is further described in detail below in conjunction with Examples 1-13 and Comparative Example 1.
[0047] raw material:
[0048] Pure acrylic emulsion Shengda Chemical S-05; phenolic epoxy resin Dahui Chemical F51; dispersant BYK-110; defoamer BYK-A530; polydiallyldimethylammonium chloride CAS: 26062-79-3; aqueous carbon nanotube dispersion Ruijiang Metal Materials 15% solid content; propylene glycol methyl ether CAS: 107-98-2; thiourea CAS: 62-56-6; diethylenetriamine CAS: 111-40-0; 4,4'-dithiodiphenylamine CAS: 722-27-0; chitosan CAS: 7447-39-4; cupric chloride CAS: 10125-13-0.
[0049] Example:
[0050] Example 1
[0051] A water-based environmentally friendly wear-resistant epoxy floor paint, the preparation method of which comprises the following steps:
[0052] S1, 100 kg of waterborne epoxy resin, 25 kg of carbon nanotube-wrapped MoO3-MoS2 nanobelts, 3 kg of dispersant BYK-110, 3 kg of defoamer BYK-A530 and 3 kg of film-forming aid-propylene glycol methyl ether were mixed at a stirring speed of 500 r / min for 1 h to obtain component A;
[0053] The preparation method of the waterborne epoxy resin is as follows: 3 kg of pure acrylic emulsion and 37 kg of phenolic epoxy resin are mixed at a stirring speed of 1000 r / min for 40 min, and then 60 kg of deionized water is added and the mixture is mixed at a stirring speed of 1000 r / min for 20 min to obtain the waterborne epoxy resin;
[0054] The preparation method of carbon nanotube-coated MoO3-MoS2 nanobelt comprises the following steps:
[0055] 1) drying the MoO3-MoS2 nanobelts and then adding them to distilled water and dispersing them at a stirring speed of 500 r / min for 30 min, wherein the mass ratio of the MoO3-MoS2 nanobelts to the distilled water is 1:5; then adding polydiallyldimethylammonium chloride and continuing to disperse them at a stirring speed of 500 r / min for 30 min to obtain a MoO3-MoS2 precursor nanobelt preparation;
[0056] 2) adding a MoO3-MoS2 precursor nanobelt preparation dropwise into a carbon nanotube dispersion, followed by filtration and drying, and then removing the dried membrane from the filter membrane, and annealing the membrane in a nitrogen environment at a temperature of 800°C, a heating rate of 10°C / min, and a holding time of 100 min to obtain a carbon nanotube-wrapped MoO3-MoS2 nanobelt;
[0057] The mass ratio of MoO3-MoS2 precursor nanobelts, polydiallyldimethylammonium chloride and carbon nanotube dispersion is 0.15:6:35;
[0058] The preparation method of MoO3-MoS2 nanobelt comprises the following steps:
[0059] A) heating MoS2 powder to 500°C in an oxygen environment, and then grinding the product to obtain nano-scale MoO3-MoS2 powder;
[0060] The particle size of MoS2 powder is 65μm, and the particle size of nano-MoO3-MoS2 powder is 650nm;
[0061] B) adding nano-sized MoO3-MoS2 powder to deionized water for dilution and stirring, the mass ratio of nano-sized MoO3-MoS2 powder to deionized water is 1:5, and then heating to 200°C for hydrothermal reaction for 72 hours. Then naturally cooling, washing, freeze-drying, and obtaining MoO3-MoS2 precursor nanobelts;
[0062] S2, 40 kg of deionized water and 30 kg of epoxy resin curing agent-diethylenetriamine were mixed at a stirring speed of 500 r / min for 1 h to obtain component B;
[0063] S3. Mix component A and component B at a stirring speed of 500 r / min for 10 min to obtain a water-based environmentally friendly floor paint, wherein the mass ratio of component A to component B is 3:1.
[0064] Example 2-3
[0065] The difference from Example 1 is that the addition amount of each component of the water-based environmentally friendly floor paint is different, as shown in Table 1:
[0066] Table 1 Addition amount of each component of water-based environmentally friendly floor paint in Examples 1-3
[0067]
[0068]
[0069] Example 4
[0070] The difference from Example 1 is that in the preparation method B) of the MoO3-MoS2 precursor nanobelts, the nanoscale MoO3-MoS2 powder is directly replaced by nanoscale MoO3 powder with the same particle size and the same addition amount.
[0071] Example 5
[0072] The difference from Example 1 is that in the preparation method 1) of carbon nanotube-wrapped MoO3-MoS2 nanobelts, polydiallyldimethylammonium chloride is no longer added.
[0073] Embodiment 6-7
[0074] The difference from Example 1 is that the mass ratios of the components in the carbon nanotube-wrapped MoO3-MoS2 nanobelts are different, as shown in Table 2:
[0075] Table 2 Mass ratio of components of MoO3-MoS2 nanobelts wrapped with carbon nanotubes in Examples 1, 6-7
[0076] Example 1 Example 6 Example 7 <![CDATA[MoO3-MoS2 precursor nanobelts]]> 0.15 0.1 0.2 Polydiallyldimethylammonium chloride 6 8 4 Carbon Nanotube Dispersion 35 40 30
[0077] Example 8
[0078] The difference from Example 1 is that in the preparation method A) of MoO3-MoS2 precursor nanobelts, the particle size of MoS2 powder is 80 μm, and the particle size of nano-scale MoO3-MoS2 powder is 500 nm.
[0079] Example 9
[0080] The difference from Example 1 is that in the preparation method A) of the MoO3-MoS2 precursor nanobelts, the particle size of the MoS2 powder is 50 μm, and the particle size of the nano-scale MoO3-MoS2 powder is 800 nm.
[0081] Example 10
[0082] The difference from Example 1 is that the epoxy resin curing agent consists of thiourea and diethylenetriamine, and the mass ratio of thiourea to diethylenetriamine is 0.45:1.
[0083] Embodiment 11
[0084] The difference from Example 10 is that the epoxy resin curing agent is composed of thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex, and the mass ratio of thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex is 0.45:1:1.3:0.3;
[0085] The preparation method of chitosan-copper chloride complex is as follows: chitosan is dissolved in a 30wt% acetic acid aqueous solution, copper chloride is subsequently added, and then precipitation and washing are performed by acetone / ethanol solvent to obtain chitosan-copper chloride complex; the mass ratio of chitosan, acetic acid aqueous solution and copper chloride is 1:5:0.3.
[0086] Examples 12-13
[0087] The difference from Example 11 is that the mass ratios of thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex are different, as shown in Table 3:
[0088] Table 3 Mass ratio of each component of epoxy resin curing agent in Examples 11-13
[0089]
[0090]
[0091] Comparative Example:
[0092] Comparative Example 1
[0093] The difference from Example 1 is that no carbon nanotubes are added to component A to wrap the MoO3-MoS2 nanobelts.
[0094] Performance testing:
[0095] 1. Wear resistance test
[0096] Three samples of 20 g were taken out from Examples 1-13 and Comparative Example 1, and then different samples were evenly applied to the planes of different cement blocks, and then cured and the original mass M0 was measured.
[0097] Then, referring to GB / T1768-2006 "Determination of abrasion resistance of paints and varnishes - Rotating rubber grinding wheel method", a 500r friction test was performed on the above samples, and then the post-test mass M1 of the samples was recorded.
[0098] Finally, the wear resistance is characterized by the wear amount, wear amount = M0-M1.
[0099] The test results are shown in Table 4:
[0100] Table 4 Wear resistance test table of Examples 1-13 and Comparative Example 1
[0101] Wear amount / g Wear amount / g Example 1 0.0006 Example 8 0.0008 Example 2 0.0012 Example 9 0.0009 Example 3 0.0013 Example 10 0.0004 Example 4 0.0024 Embodiment 11 0.0001 Example 5 0.0019 Example 12 0.0003 Example 6 0.0014 Example 13 0.0002 Example 7 0.0010 Comparative Example 1 0.0242
[0102] Referring to Examples 1-3 and Comparative Example 1 and in combination with Table 4, it can be seen that the wear resistance of Examples 1-3 is significantly improved compared with Comparative Example 1, which shows that the addition of carbon nanotube-wrapped MoO3-MoS2 nanobelts can effectively improve the wear resistance of water-based environmentally friendly epoxy floor paint.
[0103] Among them, compared with Examples 2-3, the wear resistance of Example 1 is particularly outstanding, which shows that when the components of the water-based environmentally friendly epoxy floor paint are added in the proportions of Example 1, it has better wear resistance.
[0104] With reference to Example 1 and Example 4 and in combination with Table 4, it can be seen that the wear resistance of Example 4 is significantly worse than that of Example 1, which shows that the addition of MoS2 can further improve the wear resistance of water-based environmentally friendly epoxy floor paint.
[0105] The reason is that MoS2 belongs to the hexagonal crystal system. Its crystal structure is similar to that of graphite, both of which are close-packed hexagonal structures with layered structures. Mo-S has many facets and a large specific surface area. Moreover, the layers of MoS2 are bonded to each other by weak van der Waals forces and are bonded within the layers by covalent bonds. The layers are easy to slip along the close-packed structure and are easily peeled off. It has good anisotropy and a low friction coefficient, which makes the epoxy floor paint containing MoS2 have excellent wear resistance.
[0106] Carbon nanotube-coated metal oxide has a graphene-like structure and has excellent self-lubricating properties. Similarly, carbon nanotube-coated MoO3-MoS2 nanobelts not only have self-lubricating properties, but can also effectively protect MoS2, thereby effectively reducing the possibility of further oxidation of MoS2 and further improving the wear resistance of epoxy floor paint.
[0107] Referring to Example 1 and Example 5 and combining with Table 4, it can be seen that compared with Example 1, the wear resistance of Example 5 is also significantly reduced, which shows that the addition of polydiallyldimethylammonium chloride can also improve the wear resistance of water-based environmentally friendly epoxy floor paint.
[0108] The reason is that the addition of cationic electrolyte polydiallyldimethylammonium chloride can make the surface of MoO3 positively charged, while the surface of carbon nanotube dispersion is negatively charged. After the two are mixed, the positive and negative charges attract each other. Compared with simple mechanical mixing, this method can make the carbon nanotubes tightly coated on the surface of MoO3-MoS2 precursor nanobelt preparation, further improving the wear resistance of epoxy floor paint.
[0109] With reference to Example 1, Examples 6-7 and in combination with Table 4, it can be seen that the wear resistance of Examples 6-7 is significantly reduced compared with that of Example 1. This indicates that when the components of the carbon nanotube-wrapped MoO3-MoS2 nanobelts adopt the mass proportions of the embodiments, the water-based environmentally friendly epoxy floor paint has better wear resistance.
[0110] With reference to Example 1, Examples 8-9 and in combination with Table 4, it can be seen that relative to Example 1, the wear resistance of Examples 8-9 also decreases. The reason is that, thus, when the particle size of MoS2 powder and the particle size of nano-scale MoO3-MoS2 powder adopt the parameters of Example 1, or when the ratio of MoO3 to MoS2 is in Example 1, the water-based environmentally friendly epoxy floor paint has better wear resistance.
[0111] With reference to Example 1 and Example 10 and in combination with Table 4, it can be seen that, relative to Example 1, the wear resistance of Example 10 is significantly improved, which indicates that thiourea can also improve the wear resistance of water-based environmentally friendly epoxy floor paint.
[0112] The reason is that thiourea can promote the activity of various amine-cured epoxy resins. The reason is that the nucleophilicity of the sulfur atom in thiourea is much greater than the nucleophilicity of the nitrogen atom in various amines. Compared with amines, thiourea can react with epoxy groups at a lower temperature or at a higher speed. This reaction is an exothermic reaction, which increases the temperature of the epoxy mixture near thiourea, thereby promoting the reaction of itself and various amines with epoxy groups, and then promoting the complete curing of the interior of the epoxy floor paint, effectively improving the adhesion of the epoxy floor paint, and indirectly improving the wear resistance of the epoxy floor paint.
[0113] Referring to Examples 10-11 and in combination with Table 4, it can be seen that the wear resistance of Example 11 is further improved compared with Example 10, which indicates that the addition of 4,4'-dithiodiphenylamine and chitosan-copper chloride complex can also improve the wear resistance of water-based environmentally friendly epoxy floor paint.
[0114] The reason is that 4,4'-disulfide diphenylamine is an amine curing agent containing a disulfide bond, and the disulfide bond itself has a low bond energy and is easy to break. Therefore, the disulfide bond can be easily broken and reorganized, thereby realizing a reversible dynamic exchange reaction, thereby enabling the epoxy floor paint to have a self-healing function.
[0115] In the chitosan-copper chloride complex, copper chloride has a self-repair promoting effect, while chitosan contains rich amino, acetyl and hydroxyl groups, which will interact with each other and form a diverse hydrogen bond network, thereby further improving the wear resistance of epoxy floor paint.
[0116] Referring to Examples 11-13 and in combination with Table 4, it can be seen that the wear resistance of Examples 12-13 is slightly reduced compared with Example 11, which shows that when the components of the epoxy resin curing agent adopt the proportions of Example 11, the water-based environmentally friendly epoxy floor paint has better wear resistance.
[0117] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A water-based, environmentally friendly, wear-resistant epoxy floor paint, characterized in that: The water-based environmentally friendly wear-resistant epoxy floor paint is composed of component A and component B, and the mass ratio of component A to component B is (2-4):1; The component A comprises the following raw materials in parts by weight: 90-110 parts of waterborne epoxy resin, 20-30 parts of carbon nanotube-wrapped MoO3-MoS2 nanobelts, 1-5 parts of dispersant, 1-5 parts of defoamer and 1-5 parts of film-forming aid; The method for preparing the carbon nanotube-wrapped MoO3-MoS2 nanobelt comprises the following steps: 1) drying the MoO3-MoS2 precursor nanobelt and adding it to distilled water for dispersion, and then adding polydiallyldimethylammonium chloride for further dispersion to obtain a MoO3-MoS2 precursor nanobelt preform; 2) adding a MoO3-MoS2 precursor nanobelt preparation dropwise into a carbon nanotube dispersion, followed by filtration and drying, then removing the dried membrane from the filter membrane, and annealing the membrane in a protective gas environment to obtain a carbon nanotube-wrapped MoO3-MoS2 nanobelt; The mass ratio of the MoO3-MoS2 precursor nanobelt, polydiallyldimethylammonium chloride and carbon nanotube dispersion is (0.1-0.2): (4-8): (30-40); The preparation method of the MoO3-MoS2 precursor nanobelt comprises the following steps: A) heating MoS2 powder to 400-600°C in an oxygen environment, and then grinding the product to obtain nano-scale MoO3-MoS2 powder; B) adding nano-sized MoO3-MoS2 powder to deionized water for dilution and stirring, then heating to 150-200° C. for hydrothermal reaction, then naturally cooling and washing and freeze-drying to obtain MoO3-MoS2 precursor nanobelts; The particle size of the MoS2 powder is between 50-80 μm, and the particle size of the nano-scale MoO3-MoS2 powder is between 500-800 nm; The B component includes the following raw materials in parts by weight: 30-50 parts of deionized water and 20-40 parts of epoxy resin curing agent; The epoxy resin curing agent comprises thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex, and the mass ratio of thiourea, diethylenetriamine, 4,4'-dithiodiphenylamine and chitosan-copper chloride complex is (0.3-0.6):1:(1.0-1.6):(0.2-0.4).
2. The water-based, environmentally friendly, wear-resistant epoxy floor paint according to claim 1, characterized in that: The film-forming aid is propylene glycol methyl ether.
3. A method for preparing the water-based environmentally friendly wear-resistant epoxy floor paint according to any one of claims 1-2, characterized in that: The following steps are involved: S1, mixing and stirring a water-based epoxy resin, a carbon nanotube-wrapped MoO3-MoS2 nanobelt, a dispersant, a defoaming agent and a film-forming aid to obtain a component A; S2, mixing deionized water and epoxy resin curing agent to obtain component B; S3, mixing component A and component B to obtain a water-based, environmentally friendly, wear-resistant epoxy floor paint.
Citation Information
Patent Citations
MoS2 nanoribbon and graphene composite electrode for lithium ion battery and preparation method for composite electrode
CN102709520A
Nano-composite material with molybdenum trioxide@molybdenum disulfide core-shell heterostructure, and preparation method and application thereof
CN108550805A
Self-repairing material preparing method based on duplex repairing mechanism
CN110105544A
Bi-component wear-resistant toughening modified water-borne epoxy resin floor paint and preparation method thereof
CN113292904A
Fluorinated Alkyl Ether Epoxy Resin Compositions and Applications Thereof
US20150344748A1