A magnesium / calcium borate salt and its preparation method and application

Through the reaction of low-metal active borate precursors and alcohol compounds and the high-active metal replacement method, the problems of difficulty and high cost of synthesis of raw materials by magnesium/calcium borate are solved, and high purity and high efficiency of magnesium/calcium borate are achieved. Acid preparation, suitable for high voltage battery applications.

CN116589494BActive Publication Date: 2024-11-12ZJU HANGZHOU GLOBAL SCI & TECH INNOVATION CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310236192.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-12
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

The source of synthesis raw materials for magnesium/calcium borate is difficult, the preparation cost is expensive, and the product purity in the prior art is not high and there are many by-products, which limits the development of magnesium/calcium metal batteries.

Method used

The low-metal active borate precursor is used to react with alcohol compounds, and the replacement reaction is carried out by a high-active metal magnesium or calcium to further remove residual borohydride to prepare high-purity magnesium/calcium borate.

Benefits of technology

It has achieved low cost, high yield and high purity magnesium/calcium borate preparation, excellent product performance, and is suitable for magnesium metal full battery scenarios above 3V.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589494B_ABST
    Figure CN116589494B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of metal magnesium battery or metal calcium battery, and discloses a magnesium / calcium borate salt and a preparation method and application thereof. The preparation method comprises the following steps: step 1, reacting a borohydride including metal M with an alcohol compound in a solvent to obtain a first intermediate product; wherein M is a metal element with lower activity than metal magnesium or metal calcium; step 2, reacting the first intermediate product with metal magnesium or metal calcium in a solvent to obtain a second intermediate product; step 3, reacting the second intermediate product with the alcohol compound used in step 1 to obtain the magnesium / calcium borate salt. The magnesium / calcium borate salt synthesized by the preparation method has a high purity, which can reach up to 99.85%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal magnesium batteries or metal calcium batteries, and in particular to a magnesium / calcium borate salt and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in smart phones, unmanned aerial vehicles, hybrid electric vehicles, etc., but with the development of society, traditional lithium-ion batteries are difficult to meet the needs of high-energy / high-power devices in terms of price and performance. Therefore, researchers began to study the next generation of high-energy-density metal-based batteries. Since the magnesium (~2wt%) / calcium (~3wt%) content in the earth's crust is much higher than the lithium content (0.0065%), the material cost price of metal magnesium batteries or metal calcium batteries is also much lower than the current lithium-ion battery system, but the development of these two batteries is limited by the electrolyte system.

[0003] The electrolyte materials of magnesium or calcium include magnesium salts / calcium salts of chlorine-containing Grignard reagents, Mg(BH4)2, and magnesium salts / calcium salts of carbon boron cluster anions. For example, CN 114380855 A discloses a salt containing a heteroatom compound coordinated with an anion or containing a heteroatom compound and an anion having a Lewis acid-base reaction. The radius of the central atom of the anion is large, and the steric hindrance of the negative ion bonded with it is small, so that the central atom can further coordinate with the heteroatom compound or have a Lewis acid-base reaction to change its orbital energy level, and it is easy to form a layer of inorganic magnesium ion-conducting SEI film in situ on the surface of magnesium metal, which can perform reversible magnesium deposition / dissolution, thereby inhibiting the passivation of the magnesium negative electrode and the side reaction of the magnesium negative electrode with the electrolyte. In addition, the use of chlorine-containing magnesium salts or Grignard reagent magnesium salts / calcium salts can effectively improve the deposition reversibility of magnesium metal (ACS Appl. Mater. Interfaces 2019, 11, 9062-9072), but due to the presence of a large number of free chloride ions in the electrolyte, the positive and negative electrode components and the casing of the battery are at risk of corrosion. Magnesium borohydride / calcium borohydride electrolyte salts can remove impurities on the surface of magnesium and calcium metals through borohydride ions and improve cycle reversibility, but the strong reducibility of its anions and low oxidation resistance limit its widespread use.

[0004] Among them, magnesium / calcium borate is the most commonly used electrolyte for multivalent metal magnesium / calcium batteries and has excellent performance. However, on the one hand, its synthesis method is usually prepared using raw material magnesium borohydride, but its synthetic raw materials are difficult to obtain (for example, magnesium borohydride cannot be purchased on commercial platforms since 2020), and the synthesis is complicated, making the electrolyte system costly. For example, Mg(CB 11 H 11F)2 and Mg[B(HFIP)4]2 (HFIP hexafluoroisopropoxy, -OCH(CF3)2), on the other hand, the synthesis process requires a strict experimental protocol, and some intermediates and final products are unstable under ambient conditions and decompose in the presence of moisture. This has hindered the further development of magnesium / calcium metal batteries, and the development of new magnesium / calcium borate synthesis methods is imminent.

[0005] CN105047987A discloses a chloride-free electrolyte for magnesium storage batteries and a method for converting a magnesium electrolyte into a chloride-free electrolyte, wherein the method converts water-stable borate or carborate anions into metal salts of alkali metals or silver by ion exchange and then converts them into chloride-free magnesium salts by another ion exchange. However, the end point of the exchange process is difficult to determine, the risk of magnesium halide in the product is high, and the cost of the silver element in the raw material is high, which is not easy to industrialize and recycle. Summary of the invention

[0006] The present invention aims to solve the problems of difficult sources of synthetic raw materials and high preparation costs of magnesium / calcium borates and provides a new method for preparing magnesium / calcium borates. Magnesium / calcium borates are prepared under mild conditions using low-cost raw materials and have high yield and purity. The product has excellent performance and can be applied to magnesium metal full battery scenarios above 3V.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing magnesium / calcium borate comprises the steps of:

[0009] Step 1, reacting a borohydride including a metal M with an alcohol compound in a solvent to obtain a first intermediate product; wherein M is a metal element whose activity is lower than that of metal magnesium or metal calcium; when preparing magnesium borate, the activity of M should be lower than that of metal magnesium; when preparing calcium borate, the activity of M should be lower than that of metal calcium;

[0010] Step 2, reacting the first intermediate product with metal magnesium or metal calcium in a solvent to obtain a second intermediate product; when preparing magnesium borate, metal magnesium is added; when preparing calcium borate, metal calcium is added;

[0011] Step 3, reacting the second intermediate product with the alcohol compound used in step 1 to obtain the magnesium / calcium borate.

[0012] The preparation method of magnesium borate / calcium salt provided in the present application first synthesizes a borate containing a target anion through a borate precursor with low metal activity, and then obtains an intermediate reaction product through a replacement reaction of highly active metal magnesium or calcium, and finally the second intermediate product is subjected to a secondary reaction with an alcohol compound, and the residual borohydride is further removed to obtain a pure target magnesium borate / calcium salt. In the prior art, magnesium borohydride is used to directly synthesize magnesium borate. Although the steps are relatively simple, the chloride left over from the solid phase synthesis is often residual in the raw materials, which will affect the purity of the product and the high voltage application. On the one hand, the method of the present invention can solve the shortcomings that raw materials such as magnesium borohydride or calcium borohydride are expensive, low in purity and not suitable for purchase, and on the other hand, it can solve the problem that the product purity is not high and there are more by-products.

[0013] In some embodiments, M is selected from any one of an alkaline earth metal or a transition metal.

[0014] In some embodiments, the alkaline earth metal includes beryllium or magnesium and the transition metal includes titanium, vanadium, chromium, manganese, iron, cobalt, nickel, tin, copper, or zinc.

[0015] In some embodiments, M is selected from any one of zinc, tin, beryllium, nickel, and magnesium.

[0016] When preparing calcium borate salt, magnesium borohydride can be used as a raw material, the reaction conditions are mild, there are few by-products, and the product purity is high.

[0017] In some embodiments, the borohydride of the metal M is zinc borohydride.

[0018] In some embodiments, the alcohol compound is a C1-C12 substituted or unsubstituted monohydric alcohol or polyhydric alcohol; wherein, when substituted, the substituents are each independently selected from halogens, such as fluorine, chlorine, bromine or iodine; preferably fluorine;

[0019] In some embodiments, the monohydric alcohol comprises at least one of the compounds shown in Formula I,

[0020] R1-OH Formula I

[0021] Wherein, R1 is selected from substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C7-C12 aralkyl, substituted or unsubstituted C3-C10 alicyclic hydrocarbon, substituted or unsubstituted C3-C12 heterocyclic group, preferably selected from substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C10 aryl, substituted or unsubstituted C7-C10 aralkyl, wherein, when substituted, the substituents are each independently selected from halogen, preferably fluorine;

[0022] In some embodiments, the polyol comprises at least one of the compounds of Formula II,

[0023]

[0024] Wherein, R2, R3, R4 and R5 are each independently selected from hydrogen, substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C7-C12 aralkyl, substituted or unsubstituted C3-C10 alicyclic hydrocarbon group, substituted or unsubstituted C3-C12 heterocyclic group, preferably substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C10 aryl, substituted or unsubstituted C7-C10 aralkyl, wherein, when substituted, the substituents are each independently selected from halogen, preferably fluorine; n is an integer between 0 and 6, for example, 0, 1, 2, 3, 4, 5 or 6. ;

[0025] In the present application, the C1-C10 alkyl group includes methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl or n-hexyl.

[0026] The C2-C10 alkenyl group includes vinyl, allyl, 1-propenyl, isopropenyl, 2-butenyl, 1,3-butadienyl, 3-butenyl, 4-pentenyl, 3-pentenyl, 2-hexenyl, 3-hexenyl or cyclohexenyl.

[0027] The C2-C10 alkynyl group includes ethynyl, 1-propynyl, 2-propynyl, 1,1-dimethyl-2-propynyl, 1-butynyl, 2-butynyl, 3-butynyl, 4-pentynyl, 3-pentynyl, 2-hexynyl or 3-hexynyl.

[0028] The C6-C12 aryl group includes phenyl, methylphenyl, ethylphenyl, isopropylphenyl, n-butylphenyl, isobutylphenyl, tert-butylphenyl, n-pentylphenyl, isopentylphenyl or n-hexylphenyl.

[0029] The C7-C12 aralkyl group includes a phenethyl group, a phenpropyl group, a benzyl group or a phenbutyl group.

[0030] Fluorine-substituted C1-C6 alkyl includes fluoromethyl, fluoroethyl, fluoro n-propyl, fluoro isopropyl, fluoro n-butyl, fluoro isobutyl, fluoro tert-butyl, fluoro n-pentyl, fluoro isopentyl or fluoro n-hexyl, wherein fluoro represents that at least one hydrogen atom in C1-C6 alkyl is replaced by fluorine atom. In some embodiments, fluoro-substituted C1-C6 alkyl is selected from monofluoromethyl, difluoromethyl, trifluoromethyl, difluoroethyl, trifluoroethyl, pentafluoroethyl, hexafluoro isopropyl or perfluoro tert-butyl.

[0031] Fluorine-substituted C6-C10 aryl includes fluorophenyl, fluoromethylphenyl, fluoroethylphenyl, fluoroisopropylphenyl, fluoron-butylphenyl, fluoroisobutylphenyl, fluorotert-butylphenyl, fluoron-pentylphenyl, fluoroisopentylphenyl or fluoron-hexylphenyl, wherein fluoro represents that at least one hydrogen atom in the C6-C10 aryl is replaced by a fluorine atom. In some embodiments, fluoro-substituted C6-C10 aryl is selected from monofluorophenyl, difluorophenyl, trifluorophenyl, monofluoromethylphenyl, difluoromethylphenyl, trifluoromethylphenyl, difluoroethylphenyl, trifluoroethylphenyl, pentafluoroethylphenyl, hexafluoroisopropylphenyl or perfluorotert-butylphenyl.

[0032] Fluorine-substituted C7-C10 aralkyl includes fluorophenylethyl, fluorophenylpropyl, fluorobenzyl or fluorophenylbutyl, wherein fluoro means that at least one hydrogen atom in the C7-C10 aralkyl is replaced by a fluorine atom. In some embodiments, the fluorine-substituted C7-C10 aralkyl is selected from 2-fluorobenzyl, 3-fluorobenzyl, 4-fluorobenzyl alcohol, 2,3-difluorobenzyl, 2,4-difluorobenzyl, 2,6-difluorobenzyl, 2,4,6-trifluorobenzyl, perfluorobenzyl, 4-fluorophenylethyl, 2,6-difluorophenylethyl, perfluorophenylethyl, 4-fluorophenylpropyl, 2,6-difluorophenylpropyl, perfluorophenylpropyl, 4-fluorophenylbutyl, 2,6-difluorophenylbutyl or perfluorophenylbutyl.

[0033] In some embodiments, the alcohol compound includes at least one of ethanol, trifluoroethanol, 3-fluoropropanol, 1,1,1-trifluoro-2-propanol, 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, hexafluoroisopropanol, perfluoro-tert-butyl alcohol and hexafluoro-2,3-bis(trifluoromethyl)-2,3-butanediol.

[0034] In some embodiments, the solvents in step 1 and step 2 are each independently selected from ether solvents, including one or more of ethylene glycol dimethyl ether, tetrahydrofuran, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether.

[0035] In some embodiments, in step 1, the molar ratio of the borohydride of metal M to the alcohol compound is 1:(2-10); such as 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5 or any value therebetween.

[0036] In the reaction, the molar ratio of H in the borohydride of the metal M to the hydroxyl group in the alcohol compound is 1:(0.8-1.2), which can avoid the waste of raw materials.

[0037] In some embodiments, the amount of magnesium or calcium metal added is based on the complete replacement of the metal M in the first intermediate product. In step 2, the molar ratio of magnesium or calcium metal to the borohydride of the metal M is (1-4):1; such as 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1 or any value therebetween. A slightly excess of magnesium / calcium metal can effectively replace the low-activity metal elements in the solution and improve the purity of the product.

[0038] In some embodiments, in step 3, the molar ratio of the alcohol compound to the borohydride of the metal M is (0.5-2):1; such as 1:1, 1.5:1 or any value therebetween. Adding an alcohol compound within a limited range again can further remove the residual borohydride in step 1 and improve the purity of the product.

[0039] In some embodiments, the reaction temperature of step 1 is 10-80°C, and the reaction time is 0.5-48h; such as the reaction temperature is 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C or any value therebetween, and the reaction time is 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 24h, 28h, 30h, 35h, 40h, 46h or any value therebetween. In some embodiments, when no bubbling is generated during the first reaction in step 1, it indicates that the first reaction is complete.

[0040] In some embodiments, the reaction temperature in step 2 is 10-80°C, and the reaction time is 0.5-48h; such as the reaction temperature is 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C or any value therebetween, and the reaction time is 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 24h, 28h, 30h, 35h, 40h, 46h or any value therebetween. In some embodiments, in step 2, when no solid, such as black solid, is precipitated on the metal surface during the second reaction, it indicates that the second reaction is complete.

[0041] In some embodiments, the reaction temperature of step 3 is 10-80°C, and the reaction time is 0.5-24h. For example, the reaction temperature is 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C or any value therebetween, and the reaction time is 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h or any value therebetween.

[0042] In some embodiments, the second intermediate product obtained in step 2 is filtered to remove the replaced metal, and then the reaction in step 3 is carried out.

[0043] The magnesium / calcium borate obtained in step 3 is post-treated by precipitation, centrifugation or filtration, and drying to remove the solvent to obtain pure magnesium / calcium borate;

[0044] In some embodiments, the poor solvent used for precipitation is selected from at least one of cyclohexane, n-hexane, n-pentane, and pyridine; the drying temperature is preferably 45-80° C., and the drying time is 0.5-12 hours. The volume of the precipitating agent is not less than the volume of the reaction solution to be treated.

[0045] In some embodiments, the yield of the magnesium / calcium borate salt is not less than 75%, and the purity is not less than 95%. In some embodiments, the yield is not less than 78%, 80%, 82%, 83%, 85% or any value thereof, and the purity is not less than 96%, 97%, 98%, 99% or any value therebetween.

[0046] The present invention also provides a magnesium / calcium borate, which is prepared according to the magnesium / calcium borate preparation method. The product has high purity and excellent performance, and can be applied to magnesium metal full battery scenarios above 3V.

[0047] The present invention also provides application of the magnesium / calcium borate in a secondary battery.

[0048] In some embodiments, the positive electrode material of the secondary battery includes one or more of copper sulfide, pyrene-4,5,9,10-tetraketone, and quinone materials, and the negative electrode material is metal magnesium or metal calcium.

[0049] In some embodiments, a secondary battery electrolyte includes the magnesium / calcium borate.

[0050] In some embodiments, the molar concentration of the magnesium / calcium borate salt in the electrolyte is 0.5 mol / L to 3 mol / L, or 0.5 mol / L to 2 mol / L, or 0.8 mol / L to 1.5 mol / L.

[0051] In some embodiments, the electrolyte includes a solvent, which is a commonly used solvent for electrolytes in the art, including ethylene glycol dimethyl ether (DME), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE). One or more.

[0052] In some embodiments, the liquid electrolyte may also optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance.

[0053] The present application also provides a device, which includes at least one of the above-mentioned secondary battery, battery module or battery pack.

[0054] In some embodiments, the device includes, but is not limited to: an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, a power storage system, etc. In order to meet the requirements of the device for high power and high energy density, a battery pack or a battery module may be used.

[0055] In other embodiments, the device may be a mobile phone, a tablet computer, a laptop computer, etc. The device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] The preparation method of magnesium / calcium borate provided in the present application synthesizes a borate containing a target anion through a borate precursor with low metal activity (such as Zn, Ni, Sn, Be, etc.), and then obtains the target borate through a replacement reaction of high-activity metal magnesium / calcium. This method solves the shortcomings of expensive raw materials, low purity, and inconvenient purchase. The yield and purity of the synthesized magnesium / calcium borate salt are high, and the product purity can reach up to 99.85%. The product can be directly applied to high voltage scenarios above 3V, with excellent results. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1The liquid nuclear magnetic NMR spectra of Example 1 and Example 7 are shown.

[0059] Figure 2 This is the ICP spectrum for elemental purity analysis of Example 1.

[0060] Figure 3 The liquid nuclear magnetic NMR spectra of Example 2 and Example 8 are shown.

[0061] Figure 4 The liquid nuclear magnetic NMR spectra of Example 3 and Example 9 are shown.

[0062] Figure 5 The liquid nuclear magnetic NMR spectra of Example 4 and Example 10 are shown.

[0063] Figure 6 The coulombic efficiency of the organic borate magnesium salt electrolyte synthesized in Examples 1-4.

[0064] Figure 7 The coulombic efficiency of the organic boric acid calcium salt electrolyte synthesized in Examples 7-12.

[0065] Figure 8 The 3V full battery cycle life and curve of the organic borate magnesium salt electrolyte synthesized in Example 1. DETAILED DESCRIPTION

[0066] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0067] The raw materials used in the following specific embodiments are all purchased from the market.

[0068] Example 1

[0069] Zinc borohydride Zn(BH4)2 and hexafluoroisopropanol are added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles are generated, and then metallic magnesium (molar ratio, Mg:Zn(BH4)2=1.5:1) is added to the solution to react until no black objects are precipitated on the surface of magnesium metal, and the metallic zinc is filtered to remove the reaction solution; hexafluoroisopropanol (molar ratio, hexafluoroisopropanol:Zn(BH4)2=1:1) is added thereto until no bubbles are present, and after the reaction, 2 times the volume of cyclohexane is added to the solution for precipitation, and the target salt Mg[OBHFIP]2 is obtained after filtering and drying to remove the cyclohexane.

[0070] After liquid NMR testing, the NMR spectrum is as follows Figure 1 As shown in Table 1, it can be seen that the product has high purity and no obvious impurities. Figure 2 ) and calculated, the yield was 79.3% and the purity was 99.75%. The purity and yield are summarized in Table 1.

[0071] Example 2

[0072] Zinc borohydride and perfluoro tert-butyl alcohol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic magnesium (molar ratio of Mg:Zn(BH4)2=1.5:1) was then added to the reaction solution for reaction until no black objects were precipitated on the surface of the magnesium metal, and the metallic zinc was filtered to remove the reaction solution; perfluoro tert-butyl alcohol (molar ratio: perfluoro tert-butyl alcohol:Zn(BH4)2=1:1) was added thereto until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Mg[OBpftb]2 was obtained by filtering and drying to remove the cyclohexane, and its yield and purity are shown in Table 1.

[0073] Example 3

[0074] Zinc borohydride and ethanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated to obtain a precursor, and then metallic magnesium (molar ratio of Mg:Zn(BH4)2=1.5:1) was added to the solution for reaction until no black objects were precipitated on the surface of magnesium metal, and metallic zinc was filtered to remove the reaction solution, to which ethanol (molar ratio: ethanol:Zn(BH4)2=1.5:1) was added until no bubbles were present, and after the reaction, 2 volumes of cyclohexane were added to the solution for precipitation, and the target salt Mg[OBEt]2 was obtained after filtration and drying to remove cyclohexane. The yield and purity are shown in Table 1.

[0075] Example 4

[0076] Zinc borohydride and trifluoroethanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated to obtain a precursor, and then metal magnesium (molar ratio Mg:Zn(BH4)2=1.5:1) was added to the solution for reaction until no black objects were precipitated on the surface of magnesium metal, and the metal zinc was filtered to remove the reaction solution, and trifluoroethanol (molar ratio: trifluoroethanol:Zn(BH4)2=1.5:1) was added thereto until no bubbles, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Mg[OBtfe]2 was obtained after filtering and drying to remove cyclohexane. Its yield and purity are shown in Table 1.

[0077] Example 5

[0078] Zinc borohydride and 1,1,1-trifluoro-2-propanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles were generated to obtain a precursor, and then metal magnesium (molar ratio Mg:Zn(BH4)2=1.5:1) was added to the solution for reaction until no black objects were precipitated on the surface of magnesium metal, and the metal zinc was filtered to remove the reaction solution, and 1,1,1-trifluoro-2-propanol (molar ratio: 1,1,1-trifluoro-2-propanol:Zn(BH4)2=1.5:1) was added thereto until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Mg[OBtf1p]2 was obtained after filtering and drying to remove cyclohexane. The yield and purity are shown in Table 1.

[0079] Example 6

[0080] Zinc borohydride and 3-fluoropropanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles were generated, and then metal magnesium (molar ratio Mg:Zn(BH4)2=1.5:1) was added to the solution for reaction until no black objects were precipitated on the surface of magnesium metal, and the metal zinc was filtered to remove the reaction solution, to which 3-fluoropropanol (molar ratio: 3-fluoropropanol:Zn(BH4)2=1:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Mg[OBtf2p]2 was obtained after filtering and drying to remove cyclohexane. The yield and purity are shown in Table 1.

[0081] Example 7

[0082] Zinc borohydride Zn(BH4)2 and hexafluoroisopropanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio, Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of the calcium metal, and the metallic zinc was filtered to remove the reaction solution, to which hexafluoroisopropanol (molar ratio: hexafluoroisopropanol:Zn(BH4)2=1:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBHFIP]2 was obtained after filtration and drying to remove the cyclohexane. The yield and purity are shown in Table 1.

[0083] Example 8

[0084] Zinc borohydride and perfluoro tert-butyl alcohol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio of Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of the calcium metal, and the metallic zinc was filtered to remove the reaction solution, to which perfluoro tert-butyl alcohol (molar ratio: perfluoro tert-butyl alcohol:Zn(BH4)2=1:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBpftb]2 was obtained after filtering and drying to remove the cyclohexane. The yield and purity are shown in Table 1.

[0085] Example 9

[0086] Zinc borohydride and ethanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio of Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of the calcium metal, and the metallic zinc was filtered to remove the reaction solution, to which ethanol (molar ratio: ethanol:Zn(BH4)2=1.5:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBEt]2 was obtained after filtration and drying to remove the cyclohexane. The yield and purity are shown in Table 1.

[0087] Example 10

[0088] Zinc borohydride and trifluoroethanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio of Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of the calcium metal, and the metallic zinc was filtered to remove the reaction solution, to which trifluoroethanol (molar ratio: trifluoroethanol:Zn(BH4)2=1.5:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBtfe]2 was obtained after filtration and drying to remove the cyclohexane. The yield and purity are shown in Table 1.

[0089] Embodiment 11

[0090] Zinc borohydride and 1,1,1-trifluoro-2-propanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio of Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of calcium metal. The metallic zinc was filtered to remove the reaction solution, to which 1,1,1-trifluoro-2-propanol (molar ratio: 1,1,1-trifluoro-2-propanol:Zn(BH4)2=1.5:1) was added until no bubbles were present. After the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBtf1p]2 was obtained after filtration and drying to remove cyclohexane. The yield and purity are shown in Table 1.

[0091] Example 12

[0092] Zinc borohydride and 3-fluoropropanol were added to ethylene glycol dimethyl ether solution at a molar ratio of 1:4.5, and fully reacted at 25°C for 6 hours until no bubbles were generated. Metallic calcium (molar ratio of Ca:Zn(BH4)2=1.5:1) was then added to the solution for reaction until no black objects were precipitated on the surface of the calcium metal, and the metallic zinc was filtered to remove the reaction solution, to which 3-fluoropropanol (molar ratio: 3-fluoropropanol:Zn(BH4)2=1:1) was added until no bubbles were present, and after the reaction, 2 times the volume of cyclohexane was added to the solution for precipitation, and the target salt Ca[OBtf2p]2 was obtained after filtration and drying to remove cyclohexane. The yield and purity are shown in Table 1.

[0093] Comparative Example 1

[0094] The finished product bis(trifluoromethylsulfonyl) magnesium imide Mg(TFSI)2 in the prior art is purchased from MacLean's reagent.

[0095] Comparative Example 2

[0096] The finished product calcium bis(trifluoromethylsulfonyl)imide Ca(TFSI)2 in the prior art is purchased from MacLean's reagent.

[0097] Comparative Example 3

[0098] The finished product magnesium borohydride Mg(BH4)2 in the prior art is purchased from MacLean's reagent.

[0099] The liquid NMR spectra of Mg[OBpftb]2 and Ca[OBpftb]2 obtained in Example 2 and Example 8 are as follows: Figure 3 As shown, the liquid NMR spectra of Mg[OBEt]2 and Ca[OBEt]2 prepared in Example 3 and Example 9 are as follows Figure 4 As shown, the liquid NMR spectra of Mg[OBtfe]2 and Ca[OBtfe]2 prepared in Example 4 and Example 10 are as follows Figure 5As shown, it can also be seen from each figure that the product purity is high and there are no by-products.

[0100] Application Examples

[0101] 1. Preparation of electrolyte system

[0102] Under the condition that the water oxygen content is less than 0.01 ppm, the magnesium / calcium salt obtained in Examples 1-12 is added to the ethylene glycol dimethyl ether solution, and the concentration of the magnesium / calcium salt is slowly added to 0.5 M (mol / L) to obtain the corresponding example electrolyte.

[0103] Under the condition that the water oxygen content is less than 0.01 ppm, Mg(TFSI)2 or Ca(TFSI)2 is slowly added to ethylene glycol dimethyl ether to reach 0.5 M, and the mixture is stirred evenly to obtain a comparative electrolyte.

[0104] 2. Battery preparation and decomposition voltage test

[0105] Magnesium-copper coulomb efficiency test method: Mg / Cu lithium-free negative electrode battery assembly test is used. The negative electrode shell, spring, gasket, lithium sheet, GFD glass fiber separator, copper sheet, and positive electrode shell are assembled in the order of 60-100 microliters of electrolyte are added to each battery to wet the separator, and finally the battery is packaged. The battery is first pre-charged and discharged at a current density of 0.1mA / cm2 in the 0-2V voltage range, and then deposited at a current density of 0.67mA / cm2 for 10 minutes in the 0-1.4V voltage range, and then at 0.67mA / cm 2 The lithium stripping was carried out at a current density of 1.500 N until the voltage was higher than 1.4 V, and the coulombic efficiency was calculated.

[0106] Coulomb efficiency = discharge capacity / charge capacity

[0107] Calcium-copper coulomb efficiency test method: Ca / Cu lithium-free negative electrode battery assembly test is used. The negative electrode shell, spring, gasket, lithium sheet, GFD glass fiber separator, copper sheet, and positive electrode shell are assembled in this order. 60-100 microliters of electrolyte are added to each battery to wet the separator, and the battery is finally packaged. The battery is first charged at 0.1 mA / cm in the 0–2 V voltage range. 2 The current density was used for pre-charge and discharge, and then the voltage was 2 mA / cm 2 The current density was 2 mA / cm 2 The lithium stripping was carried out at a current density of 1.50 Å until the voltage was higher than 2 V, and the coulombic efficiency was calculated.

[0108] Coulomb efficiency = discharge capacity / charge capacity

[0109] 3V magnesium metal full battery assembly method: Preparation of positive electrode sheet: The positive electrode active material pyrene-4,5,9,10-tetraketone, conductive carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in a proper amount of N-methylpyrrolidone (NMP) at a weight ratio of 3:5:2 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector Al foil to obtain a positive electrode sheet;

[0110] Preparation of negative electrode: commercial 30 micron magnesium foam; preparation of separator: 675 micron GF-D glass fiber separator is selected; preparation of magnesium metal battery: stack the positive electrode, separator and negative electrode in order, so that the separator is between the positive electrode and the negative electrode to play an isolating role, add 60-100 microliters of electrolyte to each battery to wet the separator, and finally package the battery.

[0111] 3V magnesium metal full battery test method: hang the assembled battery on the blue electric test stand, set the voltage cycle range to 1.0V-3.2V, the theoretical specific capacity is 350mAh / g, and perform charge and discharge cycles at a 4C rate. The test results are shown in Table 1. Figure 6 is the coulombic efficiency of the organic borate magnesium salt electrolyte of Examples 1-4, Figure 7 is the coulombic efficiency of the organic boric acid calcium salt electrolyte synthesized in Examples 7-12, Figure 8 The figure shows the 3V full battery cycle life and curve of the organic borate magnesium salt electrolyte synthesized in Example 1. It can be seen that the products prepared by the preparation method of the present invention have excellent performance, especially Mg[OBHFIP]2 and Mg[OBpftb]2 of Examples 1-2, which have high coulombic efficiency and long life for 3V magnesium metal batteries.

[0112] Table 1

[0113]

[0114] As can be seen from Table 1, the yield of magnesium borate / calcium salt obtained by the preparation method of the present invention is above 75%, and the purity is higher than 95%, which is much higher than the commercial magnesium borohydride in Comparative Example 3. At the same time, the cycle coulomb efficiency and number of cycles of all comparative examples are higher than those of commercial comparative examples 1 and 2.

[0115] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.

Claims

1. A method for preparing magnesium / calcium borate, characterized in that: Includes steps: Step 1, reacting zinc borohydride with an alcohol compound in a solvent to obtain a first intermediate product; the reaction temperature of step 1 is 10-80° C., and the reaction time is 0.5-48 hours; Step 2, reacting the first intermediate product with metal magnesium or metal calcium in a solvent to obtain a second intermediate product; the reaction temperature in step 2 is 10-80° C., and the reaction time is 0.5-48 hours; Step 3, reacting the second intermediate product with the alcohol compound used in step 1 to obtain the magnesium / calcium borate; the reaction temperature of step 3 is 10-80° C., and the reaction time is 0.5-24 h; The alcohol compound is at least one of ethanol, trifluoroethanol, 3-fluoropropanol, 1,1,1-trifluoro-2-propanol, 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, hexafluoroisopropanol, perfluoro-tert-butyl alcohol and hexafluoro-2,3-bis(trifluoromethyl)-2,3-butanediol; In step 1, the molar ratio of zinc borohydride to the alcohol compound is 1:(2-10); In step 2, the molar ratio of metallic magnesium or metallic calcium to zinc borohydride is (1-4):1; In step 3, the molar ratio of the alcohol compound to zinc borohydride is (0.1-2): 1 The yield of the magnesium / calcium borate salt is not less than 75%, and the purity is not less than 95%.

2. The method for preparing magnesium / calcium borate according to claim 1, characterized in that: The solvents in step 1 and step 2 are independently selected from ether solvents, which are one or more of ethylene glycol dimethyl ether, tetrahydrofuran, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether.

3. The method for preparing magnesium / calcium borate according to claim 1, characterized in that: The second intermediate product obtained in step 2 is filtered and then subjected to the reaction in step 3; And / or, the post-treatment of the magnesium / calcium borate obtained in step 3 includes precipitation, centrifugation or filtration, and drying, and the precipitating agent is selected from at least one of cyclohexane, n-hexane, n-pentane, and pyridine.