Preparation method of special resin for alkaline water electrolyzer diaphragm, product and application thereof
By adding nanozirconia and third monomers in the polymerization stage, the hydrophilicity and crystallization temperature of polyphenylene sulfide are improved, and the problems of swelling and insufficient hydrophilicity of alkaline water electrolytic cell separator materials are solved, and efficient industrialization is achieved Production.
Patent Information
- Application Number
- CN202310558929.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-18
AI Technical Summary
Existing alkaline water electrolytic cell separator materials such as asbestos swell and chemically unstable under high current loads, and the hydrophilic treatment process of alternative materials such as polyphenylene sulfide is not environmentally friendly and the equipment investment is high, making it difficult to be suitable for large-scale industrial production.
The third monomer with nanozirconia and special substituents was added during the polymerization stage. The hydrophilicity of polyphenylene sulfide was significantly improved through synergistic action, and the crystallization temperature was increased to facilitate processing by uniformly dispersing nanozirconia and reducing the average particle size. .
It significantly improves the hydrophilicity and crystallization temperature of the alkaline water electrolytic cell membrane, reduces the average particle size, improves the chemical stability and processing convenience of the material, and is suitable for industrial production.
Smart Images

Figure BDA0004234278070000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of diaphragms, and in particular to a preparation method of a special resin for diaphragms of alkaline water electrolyzers, and a product and application thereof. Background Art
[0002] Hydrogen energy, as an efficient and clean secondary energy source, has attracted widespread attention from all over the world. Large-scale and low-cost production of H2 is one of the important links in the development and utilization of H2 energy. Hydrogen production by water electrolysis has the advantages of relatively simple operation, relatively mature technology, high purity of produced H2, and no pollution in the hydrogen production process. It is an important means to achieve large-scale production of H2. At present, domestic alkaline water electrolysis dominates the water electrolysis industry.
[0003] Usually, an electrolyte (usually 20-30wt% potassium hydroxide aqueous solution) is filled in an alkaline electrolytic cell, and water is decomposed under the action of direct current, producing H2 at the cathode and O2 at the anode. The diaphragm strictly isolates the produced H2 and O2, while allowing the free movement of ions in the circuit of the electrolytic cell. The quality of the diaphragm is directly related to the purity and power consumption of H2 and O2, so it has become a hot topic of research. The requirements for the diaphragm include:
[0004] 1) It can be wetted by the electrolyte, so that the ions in the solution can pass smoothly;
[0005] 2) Good air tightness, which does not affect the safe operation of the electrolyzer and the purity of the outlet gas;
[0006] 3) Have sufficient mechanical strength;
[0007] 4) It is not corroded by alkali solution in the electrolyte and has strong chemical stability;
[0008] 5) Cheap and suitable for industrial use.
[0009] For a long time, the main raw material of alkaline electrolytic cell diaphragms has been asbestos. Asbestos diaphragms have good hydrophilic properties and easy ion permeability. However, the swelling and chemical instability of asbestos diaphragms themselves cause them to have serious swelling defects in specific operating environments, especially under high current loads, resulting in a shortened service life. Moreover, due to the limitations of the asbestos material itself, the electrolyte temperature can only be controlled below 90°C. When the electrolyte temperature exceeds 90°C, the corrosion of the asbestos diaphragm intensifies, thereby polluting the electrolyte and affecting its service life. For the above reasons, the development of new diaphragm materials that can replace asbestos diaphragms has become an important topic in the industry.
[0010] Polyphenylene sulfide (PPS) has the advantages of stable chemical properties, high temperature resistance, and resistance to harsh water electrolysis conditions such as concentrated alkali, making it a popular choice to replace asbestos diaphragms. However, PPS is highly hydrophobic and needs to be treated by grafting, oxidation, sulfonation, plasma, etc. to form a hydrophilic surface.
[0011] For example, a Chinese patent document with application publication number CN101372752A discloses a high temperature resistant alkaline water electrolyzer diaphragm and its preparation method, wherein a polyphenylene sulfide diaphragm is prepared by needle punching non-woven fabric technology, and then the PPS non-woven fabric is sulfonated and neutralized with 90-98% concentrated sulfuric acid and 30% potassium hydroxide solution in turn to improve the hydrophilicity of the non-woven fabric. Although the water absorption rate of the product prepared by this technical solution is as high as 310% or more, the production process is extremely environmentally unfriendly. Not only does it use highly corrosive raw materials such as strong acids and strong alkalis, but it also has high production risks and consumes a large amount of water resources during the post-treatment cleaning process. The cleaning time is also long, and the process operation is complicated, making it unsuitable for industrial production. At the same time, there is also the risk of fiber embrittlement and shortening the service life of the diaphragm after sulfonation treatment.
[0012] Another example is a Chinese patent document with application publication number CN 104746202 A, which discloses a diaphragm cloth for a water electrolyzer and a production method thereof, wherein polyphenylene sulfide fiber is spun through a cotton spinning process of cleaning cotton-combing cotton-drawing-roving-spinning yarn-winding-doubling yarn-twisting-heat setting, and then the obtained polyphenylene sulfide yarn is woven on a loom to obtain a high-density woven fabric; finally, hydrophilic processing is performed by plasma treatment to generate hydrophilic groups on the surface of the fabric. However, the plasma treatment used in this technical solution can only generate hydrophilic groups at a nanometer depth on the fiber surface, and this change in surface properties also has a certain effectiveness. It will gradually reduce the obtained hydrophilic groups over time, thereby causing a loss of hydrophilicity, and thus has a limited degree of improvement in the hydrophilic wettability of the material. In addition, the process equipment investment is high and is not suitable for large-scale industrial production.
[0013] Another example is a Chinese patent document with application publication number CN 113862821 A, which discloses a polyphenylene sulfate fiber fabric type alkaline water electrolysis diaphragm and a preparation method thereof, wherein inorganic zirconium oxide nanoparticles are mixed with polyphenylene sulfide resin to form granules, and then melt-spun to obtain zirconium oxide modified polyphenylene sulfide fibers, and then the fibers are spun and woven into cloth, and then subjected to a spunlace process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis diaphragm. This technical solution simply blends nano zirconium oxide with polyphenylene sulfide for modification, and it is well known that nano materials have agglomeration problems, so this method is difficult to achieve nano-scale dispersion of zirconium oxide, which in turn affects the effect of zirconium oxide on the hydrophilic modification of polyphenylene sulfide. Summary of the invention
[0014] In view of the shortcomings of the prior art, the present invention discloses a method for preparing a special resin for an alkaline water electrolyzer diaphragm. Nano zirconium oxide is added during the preparation of the resin so that the nano zirconium oxide is evenly dispersed, thereby improving the effect of hydrophilic modification of polyphenylene sulfide. A further solution is to add a third monomer with a special substituent in the polymerization stage in conjunction with the addition of the nano zirconium oxide, and utilize the synergy of the two to achieve the purpose of significantly improving the hydrophilicity of polyphenylene sulfide.
[0015] The specific technical solutions are as follows:
[0016] A method for preparing a special resin for an alkaline water electrolyzer diaphragm comprises the following steps:
[0017] Step 1: Add N-methylpyrrolidone and sodium sulfide aqueous solution into a polymerization kettle, and perform a dehydration process after heating;
[0018] Step 2: adding N-methylpyrrolidone and p-dichlorobenzene into a polymerization kettle, continuing to heat up for polymerization, and finally obtaining the alkaline water electrolyzer diaphragm special resin through a post-treatment process;
[0019] Nano zirconium oxide is also added in the preparation method. The nano zirconium oxide can be added together with the sodium sulfide aqueous solution in step one, or can be added together with p-dichlorobenzene in step two.
[0020] The preparation method disclosed in the present invention adds nano zirconium oxide in the polymerization stage of PPS resin, so that the nano zirconium oxide is evenly dispersed, thereby improving the effect of hydrophilic modification of polyphenylene sulfide. It is found through experiments that the effect of hydrophilic modification of polyphenylene sulfide is not as good as that of the present invention, compared with the case where no nano zirconium oxide is added, or when the nano zirconium oxide is added in the form of blending after the preparation of PPS resin is completed. It is also unexpectedly found through experiments that the addition of nano zirconium oxide can significantly reduce the average particle size of the prepared PPS resin and increase its crystallization temperature. With a higher crystallization temperature, it is easier to process and shape in the spinning process, and is convenient for processing.
[0021] Preferably, a third monomer is also added in step 2 of the preparation method disclosed in the present invention;
[0022] The third monomer is selected from monosubstituted p-dichlorobenzene, and the substituent is selected from one or more of sulfonic acid group, hydroxyl group, carboxylic acid group, aldehyde group and phosphoric acid group;
[0023] Experiments have shown that the addition of a third monomer can further reduce the average particle size of the prepared PPS resin and increase its crystallization temperature; and the synergistic addition of the third monomer and nano-zirconium oxide can significantly improve the hydrophilicity of the final prepared PPS-based alkaline water electrolyzer diaphragm.
[0024] Preferably, the molar ratio of the added nano zirconium oxide to sodium sulfide is 0.05-3.00:100, and the average particle size of the nano zirconium oxide is 1-100 nm.
[0025] More preferably, the molar ratio of nano zirconium oxide to sodium sulfide is 0.5-3.0:100, and the average particle size of the nano zirconium oxide is 50-100 nm.
[0026] Preferred:
[0027] The molar ratio of the third monomer to the sodium sulfide in step 1 is 0.01 to 0.5:1;
[0028] The ratio of the sum of the moles of p-dichlorobenzene and the third monomer to the mole of sodium sulfide in step 1 is 0.8 to 1.3.
[0029] Further preferably, the substituent in the third monomer is selected from one or more of a sulfonic acid group, a hydroxyl group, a carboxylic acid group, and a phosphoric acid group;
[0030] The molar ratio of the third monomer to the sodium sulfide in step 1 is 0.05-0.1:1;
[0031] The ratio of the sum of the moles of p-dichlorobenzene and the third monomer to the mole of sodium sulfide in step 1 is 1.0 to 1.2.
[0032] Further optimization:
[0033] The molar ratio of nano zirconium oxide to sodium sulfide is 0.5:100, and the average particle size of nano zirconium oxide is 50 nm;
[0034] The substituent in the third monomer is selected from sulfonic acid group and / or hydroxyl group;
[0035] The molar ratio of the third monomer to the sodium sulfide in step 1 is 0.1:1;
[0036] The ratio of the sum of the moles of p-dichlorobenzene and the third monomer to the mole of sodium sulfide in step 1 is 1.1.
[0037] With the continuous optimization of the above raw materials and process parameters, the hydrophilicity of the finally prepared PPS-based alkaline water electrolyzer diaphragm is continuously improved.
[0038] In step one:
[0039] The mass concentration of the sodium sulfide aqueous solution is 20-80%, preferably 35wt%.
[0040] The molar ratio of N-methylpyrrolidone to sodium sulfide is 1.0 to 5.0:1, preferably 2.0:1.
[0041] In step 1, the heating rate is 1-10°C / min, and the temperature is raised to 150-210°C for dehydration process;
[0042] In step 2, the temperature is raised to 240-280° C. and then polymerization is carried out, the heating rate is 1-20° C. / min, and the polymerization time is 1-8 hours;
[0043] The post-treatment includes a washing treatment and a drying treatment.
[0044] The washing process includes acetone washing and pure water washing in sequence;
[0045] The acetone washing, the molar ratio of acetone to the sodium sulfide in step 1 is 1 to 50:1, the washing times are 1 to 6 times, and the washing temperature is 10 to 40°C;
[0046] The pure water washing, the molar ratio of pure water to the sodium sulfide in step 1 is 1-100:1, the washing times are 1-10 times, and the washing temperature is 50-200°C;
[0047] The drying process is carried out at a temperature of 80 to 180° C. and for a time of 1 to 12 hours.
[0048] Preferred:
[0049] The nano zirconium oxide is added together with the sodium sulfide aqueous solution in step one; experiments have found that adding nano zirconium oxide in the dehydration stage is more conducive to reducing the average particle size of the prepared PPS resin and increasing its crystallization temperature; however, this effect is different at a lower nano zirconium oxide addition amount, and will be more significant at a higher addition amount.
[0050] The invention also discloses a special resin for alkaline water electrolyzer diaphragm prepared according to the method.
[0051] The invention also discloses a method for preparing an alkaline water electrolyzer diaphragm, which is prepared by using the alkaline water electrolyzer diaphragm-specific resin prepared by the above method as raw material through melt spinning process and needle punching non-woven fabric process.
[0052] The alkaline water electrolyzer diaphragm prepared by the invention has excellent hydrophilicity, a water absorption rate of up to 285%, and a wicking height of up to 421 mm.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] The preparation method disclosed by the invention adds nano zirconium oxide in the polymerization stage of PPS resin, so that the nano zirconium oxide is evenly dispersed, thereby improving the effect of hydrophilic modification of polyphenylene sulfide; the preparation method can also significantly reduce the average particle size of the prepared PPS resin and increase its crystallization temperature.
[0055] The present invention also discloses a preferred preparation method, in which a third monomer having a special substituent is added in the polymerization stage, which cooperates with the addition of nano zirconium oxide to not only further reduce the average particle size of the prepared PPS resin and increase its crystallization temperature, but also significantly improve the hydrophilicity of the finally prepared PPS-based alkaline water electrolyzer diaphragm. DETAILED DESCRIPTION
[0056] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0057] Example 1
[0058] Step 1: N-methylpyrrolidone (NMP), sodium sulfide aqueous solution (35wt%) and nano zirconium oxide (D50=50nm) are put into a polymerization kettle, wherein the sodium sulfide is 100mol, the NMP is 200mol, and the molar ratio of nano zirconium oxide to sodium sulfide is 0.5:100; after heating, a dehydration process is performed, the dehydration heating rate is 5°C / min, the dehydration end temperature is 180°C, and dehydration is performed until no bubbles are generated in the absorption liquid within 1 minute at the outlet of the dehydration kettle air duct;
[0059] Step 2: Add NMP, p-dichlorobenzene and the third monomer 2-hydroxy-1,4 dichlorobenzene into the polymerization kettle, the molar ratio of p-dichlorobenzene to the sodium sulfide added in step 1 is 1.05, the molar ratio of 2-hydroxy-1,4 dichlorobenzene to the sodium sulfide added in step 1 is 0.05, the NMP is 300 mol, and the polymerization is carried out after further heating. The polymerization heating rate is 5°C / min, the insulation temperature of the polymerization stage is 240°C, and the polymerization time is 4 hours.
[0060] Step 3: The product obtained in step 2 is first washed with acetone for 2 times at a washing temperature of 30°C, and the molar ratio of the resin to acetone is 50:1 each time; then washed with pure water for 5 times at a washing temperature of 80°C, and the molar ratio of the resin to pure water is 100:1 each time; finally, dried at 120°C for 6 hours to obtain a special resin for alkaline water electrolyzer diaphragm.
[0061] Comparative Example 1
[0062] The preparation process is basically the same as that of Example 1, except that nano zirconium oxide is not added in the dehydration process of step 1.
[0063] Comparative Example 2
[0064] The preparation process is basically the same as that of Example 1, except that:
[0065] No nano zirconium oxide was added in the dehydration process of step 1;
[0066] No third monomer is added in the polymerization process of step 2.
[0067] Example 2
[0068] The preparation process is substantially the same as that of Example 1, except that the third monomer added in the polymerization process of step 2 is replaced by an equimolar amount of 2-sulfonic acid-1,4-dichlorobenzene.
[0069] Example 3
[0070] The preparation process is substantially the same as that of Example 1, except that the third monomer added in the polymerization process of step 2 is replaced by an equal molar amount of 2-carboxylic acid-1,4-dichlorobenzene.
[0071] Example 4
[0072] The preparation process is substantially the same as that of Example 1, except that the third monomer added in the polymerization process of step 2 is replaced by an equimolar amount of 2-formyl-1,4-dichlorobenzene.
[0073] Example 5
[0074] The preparation process is substantially the same as that of Example 1, except that the third monomer added in the polymerization process of step 2 is replaced by an equimolar amount of 2-phospho-1,4-dichlorobenzene.
[0075] Example 6
[0076] The preparation process is basically the same as that of Example 1, except that, in the polymerization process of step 2, the molar ratio of p-dichlorobenzene to the sodium sulfide added in step 1 is 1.0:1, and the molar ratio of 2-hydroxy-1,4-dichlorobenzene to the sodium sulfide added in step 1 is 0.1:1.
[0077] Example 7
[0078] The preparation process is basically the same as that of Example 2, except that the molar ratio of nano zirconium oxide to sodium sulfide added in the dehydration process of step 1 is replaced with 0.05:100.
[0079] Example 8
[0080] The preparation process is basically the same as that of Example 2, except that the molar ratio of nano zirconium oxide to sodium sulfide added in the dehydration process of step 1 is replaced with 1.5:100.
[0081] Example 9
[0082] The preparation process is basically the same as that of Example 2, except that the molar ratio of nano zirconium oxide to sodium sulfide added in the dehydration process of step 1 is replaced with 3.0:100.
[0083] Example 10
[0084] The preparation process is basically the same as that of Example 9, except that nano zirconium oxide is not added in the dehydration process of step 1, but is added simultaneously with the third monomer in step 2, and the molar ratio of the added nano zirconium oxide to the sodium sulfide in step 1 is still 3.0:100.
[0085] Embodiment 11
[0086] The preparation process is basically the same as that of Example 2, except that the average particle size of the nano zirconium oxide added in the dehydration process of step 1 is replaced by D50=100 nm.
[0087] Example 12
[0088] The preparation process is substantially the same as that of Example 1, except that the third monomer is not added in the polymerization process of step 2.
[0089] Embodiment 13
[0090] The preparation process is basically the same as that of Example 1, except that nano zirconium oxide is not added in the dehydration process of step 1, but is added simultaneously with the third monomer in step 2, and the molar ratio of the added nano zirconium oxide to the sodium sulfide in step 1 is still 0.5:100.
[0091] The following Table 1 shows the average particle size and crystallization temperature data of the resins prepared in each embodiment and comparative example.
[0092] Table 1
[0093] serial number <![CDATA[Average particle size a / μm]]> <![CDATA[Crystallization temperature b / ℃]]> Example 1 430 225 Comparative Example 1 1300 198 Comparative Example 2 1500 193 Example 2 440 225 Example 3 445 225 Example 4 490 223 Example 5 460 224 Example 6 405 226 Example 7 1100 204 Example 8 550 222 Example 9 650 219 Example 10 670 218 Embodiment 11 560 221 Example 12 520 222 Embodiment 13 480 224
[0094] a. The average particle size is obtained by sieving test
[0095] b. The crystallization temperature was obtained by DSC testing, specifically by heating from room temperature to 380°C at a rate of 5°C / min, keeping the temperature for 5 min, and then cooling down to room temperature at a rate of 5°C / min.
[0096] Performance Test:
[0097] The resins prepared in the above-mentioned embodiments and comparative examples were melt-blended and extruded into granules by a twin-screw extruder, and then vacuum-dried at 100° C. for 12 hours and then prepared into alkaline water electrolyzer diaphragms by conventional spinning process combined with conventional needle-punched non-woven fabric process. The specific process flow is as follows:
[0098] Spinning process: granulation → drying → spinning → winding → bundling → drawing → heat setting → curling → cutting. The spinning temperature is 340℃, the ring blowing speed is 0.9m / min, the ring blowing temperature is 25℃, and the tensile heat setting temperature is 245℃.
[0099] Needle punched nonwoven fabric process: bag opener → rough opening → cotton mixing bin → fine opening → carding → web laying → needle punching → cutting. The main cylinder speed is 600m / min, and the needle punching density is 1000 needles / cm 2 , weight 550g / m 2 , needle punching winding speed 5m / min.
[0100] The alkaline water electrolyzer diaphragms prepared by spinning and needling processes using the resin raw materials of Examples 1 to 13 are numbered as samples 1 to 13; the alkaline water electrolyzer diaphragms prepared by spinning and needling processes using the resin raw materials of Comparative Examples 1 to 2 are numbered as samples 14 to 15.
[0101] The resin prepared in Comparative Example 2 was mechanically blended with nano zirconium oxide (average particle size of 50 nm), wherein the nano zirconium oxide accounted for 3% of the resin mass, and melt-blended and extruded into granules through a twin-screw extruder. The mixture was vacuum dried at 100°C for 12 hours, and then prepared into an alkaline water electrolyzer diaphragm using the aforementioned conventional spinning process combined with the conventional needle-punched non-woven fabric process, numbered as Sample 16.
[0102] The resin prepared in Comparative Example 2 was melt-extruded and granulated by a twin-screw extruder, vacuum-dried at 100° C. for 12 h, and then polyphenylene sulfide fibers were prepared according to the above spinning process, and the following surface treatment was performed on the fibers:
[0103] The polyphenylene sulfide fiber was sulfonated in 540 g / L sulfuric acid and 320 g / L chromic acid at a temperature of 80°C for 10 min. The sulfonated polyphenylene sulfide fiber was then washed with water at room temperature, washed with hot water at 50°C, reduced cleaned, and ultrasonically washed before drying to obtain hydrophilic polyphenylene sulfide fiber.
[0104] The aforementioned conventional needle-punched non-woven fabric process was then used to prepare an alkaline water electrolyzer diaphragm, numbered as sample 17.
[0105] The resin prepared in Comparative Example 2 was mechanically blended with nano zirconium oxide (average particle size of 50 nm), wherein the nano zirconium oxide accounted for 3% of the resin mass, melt blended and extruded into granules by a twin-screw extruder, vacuum dried at 100° C. for 12 h, and then polyphenylene sulfide fibers were prepared according to the above spinning process, and the following surface treatment was performed on the fibers:
[0106] The polyphenylene sulfide fiber is sulfonated in 540 g / L sulfuric acid and 320 g / L chromic acid at a temperature of 80°C for 10 min. The sulfonated polyphenylene sulfide fiber is then washed with water at room temperature, washed with hot water at 50°C, subjected to reduction cleaning, and ultrasonically washed and dried to obtain a hydrophilic polyphenylene sulfide fiber.
[0107] The aforementioned conventional needle-punched non-woven fabric process was then used to prepare an alkaline water electrolyzer diaphragm, numbered as sample 18.
[0108] All the alkaline water electrolyzer diaphragms prepared above were tested respectively, and the test data are listed in the following Table 2.
[0109] Table 2
[0110]
[0111] The applicant declares that the present invention illustrates the detailed method of the present invention through the above embodiments, but the present invention is not limited to the above detailed method.
Claims
1. A method for preparing a special resin for an alkaline water electrolyzer diaphragm, characterized in that: The steps include: Step 1: Add N-methylpyrrolidone and sodium sulfide aqueous solution into a polymerization kettle, and perform a dehydration process after heating; Step 2: adding N-methylpyrrolidone and p-dichlorobenzene into a polymerization kettle, continuing to heat up for polymerization, and finally obtaining the alkaline water electrolyzer diaphragm special resin through a post-treatment process; In step 2, a third monomer is also added; The third monomer is selected from monosubstituted p-dichlorobenzene, and the substituent is selected from one or more of sulfonic acid, hydroxyl, carboxylic acid, aldehyde, and phosphoric acid. Nano zirconium oxide is also added in the preparation method, and the nano zirconium oxide can be added together with the sodium sulfide aqueous solution in step one, or can be added together with p-dichlorobenzene in step two.
2. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: In step one: The mass concentration of sodium sulfide aqueous solution is 20~80%; The molar ratio of N-methylpyrrolidone to sodium sulfide is 1.0~5.0:
1.
3. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: The molar ratio of the added nano zirconium oxide to sodium sulfide is 0.05-3.00:100; The average particle size of the nano zirconium oxide is 1-100 nm.
4. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: The nano zirconium oxide is added together with the sodium sulfide aqueous solution in step one.
5. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: The molar ratio of the third monomer to the sodium sulfide in step 1 is 0.01-0.5:1; The ratio of the sum of the moles of p-dichlorobenzene and the third monomer to the mole of sodium sulfide in step 1 is 0.8-1.3:
1.
6. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: The substituent is selected from one or more of a sulfonic acid group, a hydroxyl group, a carboxylic acid group, and a phosphoric acid group; The molar ratio of the third monomer to the sodium sulfide in step 1 is 0.05-0.1:1; The ratio of the sum of the moles of p-dichlorobenzene and the third monomer to the mole of sodium sulfide in step 1 is 1.0-1.2:
1.
7. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 6, characterized in that: The molar ratio of the added nano zirconium oxide to sodium sulfide is 0.5-3.0:100; The average particle size of the nano zirconium oxide is 50-100 nm.
8. The method for preparing the special resin for alkaline water electrolyzer diaphragm according to claim 1, characterized in that: In step 1, the heating rate is 1-10°C / min, and the temperature is raised to 150-210°C for dehydration process; In step 2, the polymerization is carried out after the temperature is raised to 240-280°C, the heating rate is 1-20°C / min, and the polymerization time is 1-8h; The post-treatment includes a washing treatment and a drying treatment.
9. A special resin for alkaline water electrolyzer diaphragm prepared according to the method according to any one of claims 1 to 8.
10. A method for preparing a diaphragm for an alkaline water electrolyzer, characterized in that: The alkaline water electrolyzer diaphragm special resin according to claim 9 is used as a raw material and is prepared through a melt spinning process and a needle-punched non-woven fabric process.
Citation Information
Patent Citations
High temperature resistant alkaline water electrolytic cell barrier diaphragm and preparation thereof
CN101372752A
Diaphragm cloth for water electrolyser and producing method thereof
CN104746202A
Polyphenylene sulfide fiber fabric type alkaline water electrolysis diaphragm and preparation method thereof
CN113862821A
Method for preparing ultraviolet-resistant polyphenylene sulfide resin by in situ Polymerization
CN101134815A
Purification method of N-methyl pyrrolidone for high polymerization degree polyphenylene sulfide synthesis
CN103012234A
Cited By
Polyphenylene sulfide short fiber-based hydrogen production diaphragm and preparation method thereof
CN121915453A