Preparation method and application of selenium-doped manganese-cobalt bimetallic nano-spherical material

The preparation of benzonitrile by catalyzing benzonitrile oxidation by selenium-doped manganese cobalt bimetallic nanosphere material has solved the problems of high and unenvironmental catalyst cost in the prior art, and achieved a low-cost, efficient and environmentally friendly benzonitrile preparation process. Moreover, the catalyst is easy to separate and recover, and is suitable for industrial production.

CN116618067BActive Publication Date: 2024-12-06UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310617679.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

In the prior art, the catalyst for benzonitrile preparation of benzonitrile is costly and not environmentally friendly, and the problems of catalyst recovery and wastewater treatment limit industrial production, and the commonly used ruthenium-based catalyst precious metals lead to poor economic performance.

Method used

The selenium-doped manganese cobalt bimetallic nanosphere material is used as a catalyst, and benzonitrile is prepared by a simple and efficient preparation method, using oxygen or air as an oxidizing agent, which is easy to separate and recover, and the process is environmentally friendly and cheap.

Benefits of technology

It realizes low-cost and efficient benzonitrile preparation, the material has good catalytic oxidation properties, simple process, environmentally friendly, easy to separate and recycle the catalyst, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116618067B_ABST
    Figure CN116618067B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method and application of a selenium-doped manganese-cobalt bimetallic nano-spherical material. Firstly, a prepared selenium source, a cobalt source and a manganese source are added into a reaction kettle, a reaction liquid is heated for a certain time, and after cooling, an amorphous selenium-doped manganese-cobalt bimetallic catalyst is obtained by centrifugation, washing and vacuum drying. The catalyst catalyzes oxygen to oxidize benzylamine, and the conversion rate reaches more than 95%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bimetallic nanomaterial preparation, and in particular to a preparation method and application of a selenium-doped manganese-cobalt bimetallic nano spherical material. Background Art

[0002] Primary or secondary amines are easily oxidized, usually to form a series of imines, nitriles, and amides, so the selective conversion of amine oxides is very important. Benzonitrile, as an important organic intermediate, is widely used in dyes, natural products, herbicides, agricultural chemicals, pharmaceuticals, and various fine chemicals.

[0003] The common preparation methods of benzonitrile can utilize Sandmeyer reaction or toluene ammonia oxidation method. The former requires the use of stoichiometric copper, which makes it costly and environmentally unfriendly. The latter has the problem of harsh reaction conditions and easy deactivation of the catalyst. The conversion of amides, aldoximes, alcohols and amines that have been developed, especially ruthenium-based catalysts, have been proven to be effective catalysts for catalyzing the oxidation of oxygen to nitrile.

[0004] The commonly used catalyst for the oxidation of benzylamine to prepare benzonitrile is a ruthenium-based catalyst, which has mild reaction conditions and high selectivity. However, as a precious metal, ruthenium has a high cost. The recovery of the catalyst and the treatment of ruthenium-based catalyst wastewater are also major problems, which limits its application and makes it unsuitable for industrial production. Selenides are often used in semiconductor materials and have good electron transfer properties, which helps the substrate reaction oxidation.

[0005] Therefore, in order to meet the requirements of green chemistry development, it is crucial to develop new, green, efficient, recyclable and easily separable heterogeneous catalysts to use cheap and readily available oxygen or air as the final oxidant to oxidize benzylamine to prepare benzonitrile. For oxidation reactions, using oxygen or air as an oxidant has great advantages because oxygen is relatively cheap and the only byproduct produced is water, which is economical and green.

[0006] Therefore, it is very necessary to find a heterogeneous catalyst with simple process and low cost to selectively oxidize benzylamine to prepare benzonitrile. Summary of the invention

[0007] The purpose of the present invention is to provide a selenium-doped manganese-cobalt bimetallic nanomaterial and a preparation method and application thereof. The raw materials, equipment and process used in the synthesis process are simple, efficient and low-cost, and the synthesized material has good catalytic oxidation performance and has good application prospects.

[0008] The technical solution adopted by the present invention is: a method for preparing a selenium-doped manganese-cobalt bimetallic nano-spherical material, characterized in that it comprises the following steps: (1) adding selenium powder and thiourea to a reaction container, injecting hydrazine hydrate, and stirring to obtain a dark brown a solution;

[0009] (2) adding manganese salt, cobalt salt and deionized water into a reaction vessel to obtain a pink clear solution b;

[0010] (3) Transferring solution a and solution b into a reaction kettle, adding ethanol, heating, and finishing the reaction. Naturally cooling to room temperature, collecting the composition, washing, and drying to obtain selenium-doped manganese-cobalt bimetallic nano-spherical materials.

[0011] Further preferably, the manganese salt includes manganese nitrate, and the cobalt salt includes cobalt nitrate nonahydrate.

[0012] Further preferably, the molar ratio of the selenium powder, hydrazine hydrate and thiourea is 3-3.6:1-1.2:3-3.7.

[0013] Further preferably, the heating temperature is 160° C., the heating time is 20-24 h, and the volume of ethanol added is 15 ml.

[0014] The present invention also discloses a selenium-doped manganese-cobalt bimetallic nanomaterial obtained by the above-mentioned preparation method, wherein the nanomaterial is an amorphous crystalline nanoparticle.

[0015] Furthermore, the present invention also discloses the use of the selenium-doped manganese-cobalt bimetallic nanomaterial obtained by the above preparation method in catalytic oxidation of benzylamine to prepare benzonitrile. The catalytic temperature of catalytic oxidation of benzylamine to prepare benzonitrile is 130-150° C. The oxidant used is oxygen.

[0016] Compared with the prior art, the present invention has the following advantages and technical effects:

[0017] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared by the material preparation method of the present invention has nano-scale microcrystalline particles; the extremely small nano-particles can increase the contact area with the substrate, making the catalyst an active center of the oxidation reaction and accelerating the reaction.

[0018] The material obtained by the invention is prepared by a one-step alcohol thermal method, and has the advantages of simple process, low cost, environmental friendliness and high yield.

[0019] The material prepared by the invention catalyzes oxygen to oxidize benzylamine to prepare benzonitrile, and oxygen is used as the final oxidant, which is environmentally friendly and inexpensive.

[0020] The material prepared by the invention catalyzes the oxidation of benzylamine to prepare benzonitrile, and the material is easy to separate and recycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the selenium-doped manganese-cobalt bimetallic nanomaterial prepared in Example 1;

[0022] Figure 2TEM image of the selenium-doped manganese-cobalt bimetallic nanomaterial prepared in Example 1;

[0023] Figure 3 This is the HRTEM image of the selenium-doped manganese-cobalt bimetallic nanomaterial prepared in Example 1. DETAILED DESCRIPTION

[0024] Example 1

[0025] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0026] (1) Add 0.268 g (3.6 mmol) of selenium powder and 0.29 g (3.7 mmol) of thiourea to a round-bottom flask, inject 1.0 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0027] (2) Add 0.179 g (1 mmol) of manganese nitrate, 0.29 g (1 mmol) of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0028] (3) Transfer solution a into a reaction kettle, add solution a, add ethanol, heat at 160° C. for 12 h, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

[0029] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 130° C., the oxidant used is oxygen, the final conversion rate is 95.3%, and the yield is 91.2%.

[0030] The SEM, TEM and HRTEM images of the selenium-doped manganese-cobalt bimetallic nanomaterial prepared in Example 1 are shown in Figure 1 , Figure 2 , Figure 3 .

[0031] Example 2

[0032] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0033] (1) Add 0.268 g (3.6 mmol) of selenium powder and 0.29 g (3.7 mmol) of thiourea to a round-bottom flask, inject 1.2 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0034] (2) Add 0.179 g (1 mmol) of manganese nitrate, 0.58 g (2 mmol) of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0035] (3) Transfer solution a into a reaction kettle, transfer solution b into the reaction kettle, add ethanol, heat at 150° C. for 10 h, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

[0036] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 140° C., the oxidant used is oxygen, the final conversion rate is 92.1%, and the yield is 88.3%.

[0037] Example 3

[0038] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0039] (1) Add 0.233 g (3.0 mmol) of selenium powder and 0.25 g (3.2 mmol) of thiourea to a round-bottom flask, inject 1.1 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0040] (2) Add 0.358 g (2 mmol) of manganese nitrate, 0.29 g (1 mmol) of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0041] (3) Transfer solution a into a reaction kettle, transfer solution b into the reaction kettle, add ethanol, heat at 160° C. for 11 h, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

[0042] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 135° C., the oxidant used is oxygen, the final conversion rate is 95.3%, and the yield is 87.5%.

[0043] Example 4

[0044] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0045] (1) Add 0.268 g (3.6 mmol) of selenium powder and 0.29 g (3.7 mmol) of thiourea to a round-bottom flask, inject 1.2 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0046] (2) Add 0.537 g (3 mmol) of manganese nitrate, 0.58 g (2 mmol) of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0047] (3) Transfer solution a into a reaction kettle, transfer solution b into the reaction kettle, add ethanol, heat at 150° C. for 11 hours, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

[0048] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 140° C., the oxidant used is oxygen, the final conversion rate is 94.5%, and the yield is 89.7%.

[0049] Example 5

[0050] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0051] (1) Add 0.268 g (3.6 mmol) of selenium powder and 0.29 g (3.7 mmol) of thiourea to a round-bottom flask, inject 1.1 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0052] (2) Add 0.716 g (4 mmol) of manganese nitrate, 0.29 g (1 mmol) of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0053] (3) Transfer solution a into a reaction kettle, transfer solution b into the reaction kettle, add ethanol, heat at 155° C. for 11 h, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

[0054] The selenium-doped manganese-cobalt bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 130° C., the oxidant used is oxygen, the final conversion rate is 95.1%, and the yield is 88.2%.

[0055] Comparative Example 1

[0056] A method for preparing selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps:

[0057] (1) Add 3.6 mmol of selenium powder and 3.7 mmol of thiourea to a round-bottom flask, inject 1.1 mmol of hydrazine hydrate, and stir for 2 hours to obtain a dark brown solution a;

[0058] (2) Add 4 mmol of ferric nitrate, 1 mmol of cobalt nitrate hexahydrate, and 10 ml of deionized water into a round-bottom flask to obtain a pink clear solution b;

[0059] (3) Transfer solution a into a reaction kettle, transfer solution b into the reaction kettle, add ethanol, heat at 155° C. for 11 h, and after the reaction is completed, cool naturally to room temperature, collect the composition, wash, and dry to obtain the bimetallic nanomaterial.

[0060] The bimetallic nanomaterial prepared under the conditions described in this example catalyzes oxygen oxidation of benzylamine to prepare benzonitrile, wherein the reaction temperature is 130° C., the oxidant used is oxygen, and the final benzylamine conversion rate is 82.4% and the yield is 73.9%.

[0061] The detailed description of a selenium-doped manganese-cobalt bimetallic nanomaterial and its preparation method and application with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.

Claims

1. An application of selenium-doped manganese-cobalt bimetallic nanomaterial in catalytic oxidation of benzylamine to prepare benzonitrile, characterized in that: The preparation method of the selenium-doped manganese-cobalt bimetallic nanomaterial comprises the following steps: (1) Add selenium powder and thiourea to a reaction vessel, inject hydrazine hydrate, and stir to obtain a dark brown solution a, wherein the molar ratio of the selenium powder, hydrazine hydrate, and thiourea is 3-3.6:1-1.2:3-3.7; (2) adding a manganese salt, a cobalt salt and deionized water into a reaction container to obtain a pink clear solution b, wherein the manganese salt is manganese nitrate and the cobalt salt is cobalt nitrate hexahydrate; (3) Transferring solution a and solution b into a reaction kettle, adding ethanol, heating, and completing the reaction. Naturally cooling to room temperature, collecting the composite, washing, and drying to obtain selenium-doped manganese-cobalt bimetallic nanomaterials.

2. The use according to claim 1, characterized in that: The heating temperature in step (3) is 150-160° C., and the heating time is 10-12 h.

3. The use according to claim 1, characterized in that: The selenium-doped manganese-cobalt bimetallic nanomaterial is stacked crystalline nanoparticles in irregular shapes.

4. The use according to claim 1, characterized in that: The catalytic temperature of the catalytic oxidation of benzylamine to prepare benzonitrile is 130-140°C.

5. The use according to claim 1, characterized in that: In the catalytic oxidation of benzylamine to prepare benzonitrile, oxygen is used as an oxidant.