Titanium dioxide-ruthenium oxide composite nanofiber material and preparation method and application thereof

The titanium dioxide-ruthenium oxide composite nanofiber material prepared by electrospinning and calcining methods solved the problem of the influence of impurities in seawater, achieved efficient photocatalytic decomposition of water in seawater, and demonstrated excellent hydrogen production performance and stability.

CN116637609BActive Publication Date: 2024-11-15CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310595058.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-15
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing photocatalytic decomposition of water hydrogen production technology mainly uses pure water, which ignores the potential of seawater. The impurity ions in seawater have a serious impact on the photocatalytic reaction, resulting in unstable photocatalyst performance.

Method used

The titanium dioxide-ruthenium oxide composite nanofiber material is prepared by electrospinning and calcining method. By adjusting the amount of ruthenium source and calcining conditions, a close-contact interface between titanium dioxide and ruthenium oxide is formed, and ruthenium oxide is used as a cocatalyst to separate electrons and holes. Improve photocatalytic performance.

Benefits of technology

It exhibits excellent hydrogen production performance in simulated seawater, which can be comparable to pure water systems, reduces the influence of impurity ions, improves electron-hole separation efficiency, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116637609B_ABST
    Figure CN116637609B_ABST
Patent Text Reader

Abstract

The present invention provides a titanium dioxide-ruthenium oxide composite nanofiber material and its preparation method and application. The method uses titanium dioxide nanofiber as a carrier, adds a ruthenium source to the spinning solution at the same time to prepare a mixed solution, and prepares the composite nanofiber in situ by high-voltage electrospinning and high-temperature calcination. The in-situ grown ruthenium oxide consumes holes in the titanium dioxide photocatalyst as an oxidative co-catalyst, effectively separates electrons and holes, and promotes the reduction reaction. Composite nanofibers with excellent hydrogen production performance in simulated seawater are prepared by adjusting the amount of ruthenium source in the spinning mixed solution, and its hydrogen production performance is comparable to that of a pure water system. In the process of using seawater to produce hydrogen, ruthenium oxide receives holes in the titanium dioxide valence band, improves the electron-hole separation efficiency, and synergistically simulates Cl-consumption holes in seawater, promotes the separation of electrons and holes, and avoids the adverse effects of impurity ions in simulated seawater on hydrogen evolution activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photocatalytic material synthesis technology and application, and specifically relates to titanium dioxide-ruthenium oxide composite nanofiber material and a preparation method and application thereof. Background Art

[0002] As an emerging energy technology, photocatalytic water decomposition technology for hydrogen production has attracted widespread attention from researchers. Hydrogen has a high calorific value and its combustion products are pollution-free, making it undoubtedly a friendly new energy source. Photocatalytic water decomposition technology for hydrogen production can effectively obtain clean energy using sustainable solar energy as a power source. At present, research on photocatalytic hydrogen production mainly focuses on the design of photocatalysts, almost all of which use pure water as a medium, while ignoring the use of other media. However, nearly 97.5% of the water resources on the earth are seawater, and most of the fresh water still exists on the earth in the form of ice sheets or groundwater. Considering the shortage of fresh water resources on the earth, directly using seawater to produce hydrogen without the need for water purification equipment can greatly reduce production costs. However, current research on seawater hydrogen production mainly focuses on electrocatalysis. Compared with electrocatalytic seawater technology, photocatalysis has the characteristics of green and energy-saving. Therefore, it is particularly important to conduct in-depth research on the reaction process of photocatalytic decomposition of seawater. According to previous studies, sodium ions (Na + ), magnesium ion (Mg 2+ ), calcium ions (Ca 2+ ), potassium ion (K + ), chloride ion (Cl - ) and sulfate ions account for more than 99% of the total salt content of seawater, which seriously affects the photocatalytic reaction. How to avoid the influence of impurity ions in seawater on the photocatalytic reaction and design a suitable, stable and high-performance photocatalyst is particularly important. Summary of the invention

[0003] The purpose of the present invention is to provide a titanium dioxide-ruthenium oxide composite nanofiber material and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] The first object of the present invention is to provide a method for preparing a titanium dioxide-ruthenium oxide composite nanofiber material, wherein the titanium dioxide-ruthenium oxide composite nanofiber material is prepared by an electrospinning method and a calcination method, and comprises the following specific steps:

[0006] Step S1, preparation of nanofiber precursor solution: uniformly mixing a titanium source and an organic solvent, adding a spinning aid and a ruthenium source, stirring and mixing to obtain a mixed solution, and subjecting the mixed solution to an electrostatic spinning method to obtain a nanofiber precursor solution;

[0007] Step S2, calcination treatment: calcining the nanofiber precursor solution prepared in step S1 to obtain titanium dioxide-ruthenium oxide composite nanofibers.

[0008] Furthermore, in step S1, the organic solvent includes ethanol and acetic acid, the mass ratio of the titanium source, ethanol and acetic acid is 1:4:1 to 1:6:1, and the added amount of the ruthenium source is 0.2% to 3% of the mass of the titanium source.

[0009] Furthermore, during the electrospinning process, the distance between the spinning needle and the receiving plate is maintained at 10 to 20 cm, the voltage is 10 to 20 kV, and the spinning rate is 1.0 to 3.0 mL / h.

[0010] Furthermore, the titanium source includes at least one of tetrabutyl titanate, isopropyl titanate and tetraethyl titanate.

[0011] Furthermore, the ruthenium source includes at least one of ruthenium carbonate, ruthenium chloride, ruthenium acetate, ruthenium sulfate and ammonium hexachlororuthenate.

[0012] Furthermore, in step S2, the calcination process is to continuously increase the temperature to 400-600°C at a heating rate of 1-3°C / min and maintain it for 2-4h.

[0013] The second object of the present invention is to provide a titanium dioxide-ruthenium oxide composite nanofiber material prepared by the above method.

[0014] Furthermore, the diameter of the titanium dioxide-ruthenium oxide composite nanofiber material is 100-200 nm.

[0015] The third object of the present invention is to provide the application of the above titanium dioxide-ruthenium oxide composite nanofiber material in photocatalytic water decomposition to produce hydrogen.

[0016] The fourth object of the present invention is to provide a method for producing hydrogen using seawater, using a xenon lamp as a light source and the above-mentioned titanium dioxide-ruthenium oxide composite nanofiber material to reduce H2O in seawater into H2.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) The titanium dioxide-ruthenium oxide composite nanofiber material and its preparation method provided by the present invention. The method uses titanium dioxide nanofiber as a carrier, adds a ruthenium source to the spinning solution of titanium dioxide fiber to prepare a mixed solution, and uses high-voltage electrospinning and high-temperature calcination to in situ prepare composite nanofibers with uniform morphology, smooth surface and a diameter of about 100 to 200 nm, thereby forming a closer contact interface between titanium dioxide and ruthenium oxide, which fully contacts with water molecules in simulated seawater for hydrogen production reaction. By adjusting the amount of ruthenium source in the spinning mixed solution, composite nanofibers with excellent hydrogen production performance in simulated seawater are prepared, and their hydrogen production performance is comparable to that of a pure water system. Among them, the in situ grown ruthenium oxide acts as an oxidative co-catalyst to consume holes in the titanium dioxide photocatalyst, effectively separate electrons and holes, and promote the reduction reaction.

[0019] (2) The method of the present invention has simple procedures, convenient operation, readily available raw materials, no need for complex equipment, low production cost, and is very suitable for large-scale industrial production.

[0020] (3) In the titanium dioxide-ruthenium oxide composite nanofiber material provided by the present invention, titanium oxide is an oxidative photocatalyst and ruthenium oxide is a hole consumption auxiliary agent. Under light conditions, the electrons in the valence band of the titanium dioxide-ruthenium oxide composite nanofiber material are excited to the conduction band, and ruthenium oxide, as an oxidative auxiliary agent, effectively transfers the holes in the valence band of TiO2, effectively promotes the electron-hole separation inside the photocatalyst, and retains the electrons in the conduction band of TiO2 to participate in the reduction reaction and generate hydrogen.

[0021] (4) In the process of using seawater to produce hydrogen, the titanium dioxide-ruthenium oxide composite nanofiber material provided by the present invention receives holes in the valence band of titanium dioxide, thereby improving the electron-hole separation efficiency and acting as a good oxidation promoter to synergistically simulate the Cl in seawater. - The consumption of holes promotes the separation of electrons and holes, thus avoiding the adverse effects of impurity ions in simulated seawater on hydrogen evolution activity. - By participating in the consumption of holes, it is expected to generate sodium hypochlorite with high added value, and synergistically act with ruthenium oxide to improve the electron-hole separation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] FIG1 is a scanning electron microscope photograph of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention;

[0023] Figure 2 The X-ray diffraction pattern of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention;

[0024] Figure 3This is a transmission electron microscope image of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the invention;

[0025] Figure 4 This is a high-resolution X-ray photoelectron spectrum of Ru 3d in the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention;

[0026] Figure 5 The steady-state fluorescence image of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention, wherein the prepared titanium dioxide-ruthenium oxide composite nanofiber is simply named TR-0.5% according to the theoretical mass ratio of the ruthenium source to titanium dioxide being 0.5%;

[0027] Figure 6 This is a transient fluorescence image of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention, wherein, according to the theoretical mass ratio of the ruthenium source to titanium dioxide being 0.5%, the prepared titanium dioxide-ruthenium oxide composite nanofiber is simply named TR-0.5%;

[0028] Figure 7 The UV-visible diffuse reflectance spectra of the titanium dioxide-ruthenium oxide composite nanofiber materials prepared in Examples 1-4 of the present invention, wherein the prepared titanium dioxide-ruthenium oxide composite nanofibers are simply named TR-x% according to the different theoretical weights of titanium dioxide occupied by the ruthenium source;

[0029] Figure 8 The photocatalytic hydrogen production mechanism diagram of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1 of the present invention by simulating seawater;

[0030] Fig. 9 The hydrogen evolution performance diagram of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Examples 1-4 of the present invention in simulated seawater, wherein the prepared titanium dioxide-ruthenium oxide composite nanofiber material is simply named TR-x% according to the different theoretical mass of titanium dioxide occupied by the ruthenium source;

[0031] Fig.10 This is a graph showing the hydrogen evolution performance of the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Examples 9-16 and Comparative Examples 3-4 of the present invention in simulated seawater. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are further described in detail below in conjunction with specific examples and drawings. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0033] Example 1

[0034] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0035] Step S1, preparation of nanofiber precursor:

[0036] A certain amount of ethanol, acetic acid and tetrabutyl titanate (TBT) were mixed and stirred for a certain period of time, and then 0.75g of polyvinyl pyrrolidone (PVP) and ruthenium trichloride were added, and the amount of ruthenium trichloride added was 0.5% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 10 hours; the mass ratio of TBT, ethanol and acetic acid was 1:5:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV, and the solution propulsion speed was set to 2.0mL / h, and after the mixed solution was propulsion completed, the nanofiber precursor was collected on the receiving plate;

[0037] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 550°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0038] As shown in Figures 1(a) and 1(b), the scanning electron microscope images of titanium dioxide and titanium dioxide-ruthenium oxide composite nanofibers prepared in Example 1 are shown, wherein Figure 1(b) is an enlarged scanning electron microscope image of titanium dioxide nanofibers. As shown in the figure, both titanium dioxide and titanium dioxide-ruthenium oxide composite nanofibers exhibit a smooth nanofiber morphology with a diameter of about 100 to 200 nm.

[0039] like Figure 2Shown are the X-ray diffraction patterns of titanium dioxide and titanium dioxide-ruthenium oxide composite nanofibers prepared in this embodiment. Among them, the diffraction peaks are located at 25.46°, 38.00°, 48.47° and 62.90°, which match the (101), (103), (200) and (213) crystal planes of anatase phase TiO2 (JCPDS Card No.1-562). The remaining diffraction peaks are located at 27.61°, 36.03°, 54.17°, 56.91° and 69.16°, which match the (110), (101), (211), (220) and (301) crystal planes of rutile phase (JCPDS Card No.1-1292). The diffraction peaks of the composite material are similar to those of TiO2. The difference is that during the high-temperature calcination process, the in-situ growth process of ruthenium oxide affects the grain growth of TiO2, resulting in the intensity change of its diffraction peak at 27.61°. In addition, with the increase of ruthenium oxide content, the diffraction peak belonging to ruthenium oxide is detected at 35.32°. In addition, no diffraction peak signals of other substances are detected, proving that there are no other impurities in the entire system.

[0040] like Figure 3 The figure shows the transmission electron microscope spectra of titanium dioxide and titanium dioxide-ruthenium oxide composite nanofibers prepared in this example. Figure 3 (a) It can be seen that the nanofiber morphology in the low-magnification transmission spectrum of titanium dioxide-ruthenium oxide composite nanofibers is consistent with the scanning electron microscope, showing a uniform nanofiber morphology with a diameter of about 100 to 200 nm. Figure 3 (b) It can be seen that in the high-magnification transmission spectrum of titanium dioxide-ruthenium oxide composite nanofibers, lattice spacings of 0.32nm and 0.24nm belonging to rutile titanium dioxide and 0.35nm belonging to anatase titanium dioxide were detected. Due to the small amount of ruthenium source added, the presence of ruthenium oxide in the composite nanofibers was confirmed by X-ray photoelectron spectroscopy (XPS) testing.

[0041] like Figure 4 The figure shows the high-resolution XPS spectrum of Ru element in the titanium dioxide-ruthenium oxide composite nanofibers prepared in this example. It can be seen that the peaks of 282.33 and 286.07 eV in Ru 3d belong to Ru. IV O2 oxidation state, further confirming the successful preparation of the composite nanofibers. At the same time, the X-ray energy dispersive instrument equipped with XPS performed a semi-quantitative analysis of the element content. Ti, O, and Ru elements were present in the titanium dioxide-ruthenium oxide composite nanofibers, of which the O element content was 69.06%, the Ti element content was 30.76%, and the Ru element content was 0.18%, indicating the successful preparation of the composite nanofibers.

[0042] like Figure 5 and Figure 6 The steady-state fluorescence spectrum and transient fluorescence spectrum of the titanium dioxide-ruthenium oxide composite nanofiber prepared in this example are shown in FIG. Figure 5 It can be seen that titanium dioxide nanofibers show two obvious emission peaks at an excitation wavelength of 280nm. Among them, the emission peak at 387nm can be attributed to the band gap transition between anatase and rutile phases of titanium dioxide, while the emission peak at 466nm is caused by the free excitons at the band edge. The steady-state fluorescence intensity of titanium dioxide-ruthenium oxide composite nanofibers is significantly lower than that of titanium dioxide, indicating that the introduction of ruthenium oxide can effectively capture holes in the valence band of titanium dioxide and inhibit electron-hole recombination. Figure 6 It can be seen that in the transient fluorescence spectrum, the average lifetime of titanium dioxide-ruthenium oxide composite nanofibers is significantly extended compared with titanium dioxide after fitting the transient fluorescence spectrum data using a double exponential decay kinetic function. Among them, the short lifetime (τ1) and the long lifetime (τ2) represent the radiation and non-radiation combination paths, respectively. In titanium dioxide-ruthenium oxide composite nanofibers, the decrease in the long lifetime percentage (A2) and the increase in the short lifetime percentage (A1) reveal the effective separation and transfer of carriers in the composite nanofibers.

[0043] Example 2

[0044] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0045] Step S1, preparation of nanofiber precursor:

[0046] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.6g of polyvinyl pyrrolidone (PVP) and ruthenium trichloride were added, and the amount of ruthenium trichloride added was 0.25% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 12 hours; the mass ratio of TBT, ethanol and acetic acid was 1:3:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 10kV, and the solution propulsion speed was set to 3.0mL / h, and after the mixed solution was propulsed, the nanofiber precursor was collected on the receiving plate;

[0047] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 550°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0048] Example 3

[0049] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0050] Step S1, preparation of nanofiber precursor:

[0051] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.9g of polyvinyl pyrrolidone (PVP) and ruthenium trichloride were added, and the amount of ruthenium trichloride added was 1% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 15 hours; the mass ratio of TBT, ethanol and acetic acid was 1:4:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV, and the solution propulsion speed was set to 1.0mL / h, and after the mixed solution was propulsion completed, the nanofiber precursor was collected on the receiving plate;

[0052] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 550°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0053] Example 4

[0054] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0055] Step S1, preparation of nanofiber precursor:

[0056] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 1.0g of polyvinyl pyrrolidone (PVP) and ruthenium trichloride were added, and the amount of ruthenium trichloride added was 2% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 10 hours; the mass ratio of TBT, ethanol and acetic acid was 1:6:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 15kV, and the solution propulsion speed was set to 2.0mL / h, and after the mixed solution was propulsion completed, the nanofiber precursor was collected on the receiving plate;

[0057] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 550°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0058] Example 5

[0059] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0060] Step S1, preparation of nanofiber precursor:

[0061] A certain amount of ethanol, acetic acid and tetraethyl titanate were mixed and stirred for a certain period of time, and then 0.75g of polyvinyl alcohol and ruthenium carbonate were added, the mass of ruthenium carbonate was 0.5% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 12 hours; the mass ratio of tetraethyl titanate, ethanol and acetic acid was 1:5:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV and the propulsion speed of the solution was set to 2.0mL / h, and after the mixed solution was propulsed, the nanofiber precursor was collected on the receiving plate;

[0062] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 600°C at a heating rate of 1°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, namely titanium dioxide-ruthenium oxide composite nanofibers.

[0063] Example 6

[0064] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0065] Step S1, preparation of nanofiber precursor:

[0066] A certain amount of ethanol, acetic acid and tetraisopropyl titanate were mixed and stirred for a certain period of time, and then 0.75g of polyethylene glycol and ruthenium acetate were added, the mass of ruthenium acetate was 0.5% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 10 hours; the mass ratio of tetraisopropyl titanate, ethanol and acetic acid was 1:5:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV, the propulsion speed of the solution was set to 2.0mL / h, and after the mixed solution was propulsed, the nanofiber precursor was collected on the receiving plate;

[0067] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 400°C at a heating rate of 3°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0068] Example 7

[0069] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0070] Step S1, preparation of nanofiber precursor:

[0071] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.75g of polyglycolic acid and ruthenium sulfate were added, the mass of ruthenium sulfate was 0.5% of the theoretical mass of TiO2, and continued to stir vigorously at room temperature for 10 hours; the mass ratio of TBT, ethanol and acetic acid was 1:5:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV, the solution propulsion speed was set to 2.0mL / h, and after the mixed solution was propulsion completed, the nanofiber precursor was collected on the receiving plate;

[0072] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 550°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0073] Example 8

[0074] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this embodiment are as follows:

[0075] Step S1, preparation of nanofiber precursor:

[0076] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.75g of polyvinyl pyrrolidone (PVP) and ammonium hexachlororuthenate were added, and the mass concentration of the ruthenium source was 0.5% of the theoretical mass of TiO2. The mixture was stirred vigorously for 10 hours at room temperature. The mass ratio of TBT, ethanol and acetic acid was 1:5:1. The obtained brown solution was injected into a 20mL syringe, and the distance between the spinning needle and the receiving plate was kept at 10cm. The voltage was set to 20kV, and the propulsion speed of the solution was set to 3.0mL / h. After the mixed solution was propulsed, the nanofiber precursor was collected on the receiving plate.

[0077] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 600°C at a heating rate of 3°C / min in an air atmosphere and maintained for 2 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0078] Comparative Example 1

[0079] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this comparative example are as follows:

[0080] Step S1, preparation of nanofiber precursor:

[0081] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.75g of polyvinyl pyrrolidone (PVP) and ruthenium trichloride were added, the mass of ruthenium trichloride was 0.1% of the theoretical mass of TiO2, and the mixture was stirred vigorously for 10 hours at room temperature; the mass ratio of TBT, ethanol and acetic acid was 1:5:1; the obtained brown solution was injected into a 20mL syringe, the distance between the spinning needle and the receiving plate was kept at 10cm, the voltage was set to 20kV, the propulsion speed of the solution was set to 2.0mL / h, and the nanofiber precursor was collected on the receiving plate after the mixed solution was propulsed;

[0082] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 800°C at a heating rate of 2°C / min in an air atmosphere and maintained for 5 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0083] Comparative Example 2

[0084] The steps of the preparation method of the titanium dioxide-ruthenium oxide composite nanofiber material provided in this comparative example are as follows:

[0085] Step S1, preparation of nanofiber precursor:

[0086] A certain amount of ethanol, acetic acid and TBT were mixed and stirred for a certain period of time, and then 0.75g of polyvinyl pyrrolidone (PVP) and ammonium hexachlororuthenate were added, and the mass concentration of the ruthenium source was 0.1% of the theoretical mass of TiO2. The mixture was stirred vigorously for 10 hours at room temperature. The mass ratio of TBT, ethanol and acetic acid was 1:5:1. The obtained brown solution was injected into a 20mL syringe, and the distance between the spinning needle and the receiving plate was kept at 10cm. The voltage was set to 20kV, and the propulsion speed of the solution was set to 2.0mL / h. After the mixed solution was propulsed, the nanofiber precursor was collected on the receiving plate.

[0087] Step S2, calcination treatment: the nanofiber precursor sample obtained in step S1 is continuously heated to 350°C at a heating rate of 2°C / min in an air atmosphere and maintained for 5 hours to obtain light brown nanofibers, that is, titanium dioxide-ruthenium oxide composite nanofiber material.

[0088] like Figure 7 Shown is the ultraviolet diffuse reflection absorption spectrum of titanium dioxide-ruthenium oxide composite nanofibers in Examples 1-4. As can be seen from the figure, the light absorption capacity of titanium dioxide-ruthenium oxide composite nanofibers is significantly improved compared to titanium dioxide nanofibers. The improvement of the light absorption performance of the photocatalyst can promote the absorption of light and further promote the photocatalytic hydrogen production reaction. The absorption band edge of the composite nanofiber moves to the high absorption range, indicating that the introduction of ruthenium oxide leads to changes in the energy band structure of the sample.

[0089] In order to better illustrate the effect of the titanium dioxide-ruthenium oxide composite nanofibers of the present invention in hydrogen production using seawater, the applicant conducted the following research:

[0090] The photocatalytic simulated seawater hydrogen production test experiment was carried out in a 60mL quartz glass bottle with a 300W xenon lamp as the light source. The distance between the light source and the quartz glass bottle was about 10cm. The prepared titanium dioxide-ruthenium oxide composite nanofibers were placed in the quartz bottle, and a simulated seawater solution (inorganic salt) and a sacrificial reagent were added as solvents. Before the illumination experiment, nitrogen was passed into the bottle for more than 30 minutes to remove the air in the bottle to ensure that the entire system remained in an inert gas state before the illumination reaction. Furthermore, the illumination reaction was carried out under illumination and stirring. After a certain reaction time, a certain amount of gas was extracted from the bottle, and the hydrogen content was detected by gas chromatography using the external standard method.

[0091] The gas chromatograph used was Shimadzu GC2014C, with nitrogen as carrier gas, column flow rate of 20.0 mL / min, column temperature of 70 ° C, and detector temperature of 100 ° C. The chromatographic column used was a stainless steel packed column, the filler was 5A molecular sieve, the length was 5 m, and the inner diameter was 2.00 mm.

[0092] like Figure 8 The diagram shows the mechanism of the photocatalytic hydrogen production of titanium dioxide-ruthenium oxide composite nanofibers in a simulated seawater system. Under light conditions, the electrons in the valence band of the photocatalyst are excited to the conduction band, and ruthenium oxide, as an oxidizing agent, effectively transfers the holes in the valence band of TiO2, effectively promoting the electron-hole separation inside the photocatalyst, and retains the electrons in the conduction band of TiO2 to participate in the reduction reaction and generate hydrogen. In addition, the Cl - By participating in the consumption of holes, it is expected to generate sodium hypochlorite with high added value, and synergistically act with ruthenium oxide to improve the electron-hole separation efficiency.

[0093] Example 9

[0094] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 1:

[0095] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with a NaCl (0.6 M)-methanol aqueous solution (30%) and stirring them evenly;

[0096] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0097] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0098] Example 10

[0099] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 2:

[0100] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with a NaCl (0.6 M)-methanol aqueous solution (30%) and stirring them evenly;

[0101] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0102] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0103] Embodiment 11

[0104] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 3:

[0105] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl (0.6 M)-methanol aqueous solution (30%) and stirring them evenly;

[0106] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0107] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0108] Example 12

[0109] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 4:

[0110] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl (0.6 M)-methanol aqueous solution (30%) and stirring them evenly;

[0111] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0112] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0113] Example 13

[0114] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 5:

[0115] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with NaCl-MgCl2 (0.2M)-triethanolamine aqueous solution (20%) and stirring them evenly;

[0116] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0117] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0118] Embodiment 14

[0119] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 6:

[0120] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl-MgCl2 (0.3 M)-triethanolamine aqueous solution (10%) and stirring them evenly;

[0121] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0122] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0123] Embodiment 15

[0124] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 7:

[0125] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl-CaSO4 (0.4 M)-methanol aqueous solution (40%) and stirring them evenly;

[0126] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0127] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0128] Example 16

[0129] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Example 8:

[0130] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl-K2SO4 (0.5 M)-methanol aqueous solution (30%) and stirring them evenly;

[0131] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0132] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0133] Comparative Example 3

[0134] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Comparative Example 1:

[0135] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl-MgCl2 (0.6 M)-methanol aqueous solution (20%), and stirring the mixture to obtain a uniform mixture;

[0136] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0137] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0138] Comparative Example 4

[0139] The simulated seawater hydrogen production test using the titanium dioxide-ruthenium oxide composite nanofiber material prepared in Comparative Example 2:

[0140] a) weighing 10 mg of titanium dioxide-ruthenium oxide composite nanofibers and mixing them with 30 mL of NaCl (0.6 M)-methanol aqueous solution (20%) and stirring them evenly;

[0141] b) Use nitrogen to continuously ventilate the quartz reaction bottle for 30 minutes to remove the air in the bottle for hydrogen detection;

[0142] c) Use a xenon lamp as the light source to perform a photoreaction. Extract a certain amount of gas every hour and use gas chromatography to detect hydrogen.

[0143] like Fig. 9Shown is a graph comparing the hydrogen production performance of Examples 9-12. In the figure, the theoretical mass ratio of ruthenium oxide to titanium dioxide is simply marked as TR-0.25%, TR-0.5%, TR-1% and TR-2%. According to the different mass ratios of ruthenium oxide, the photocatalytic hydrogen production performance of the titanium dioxide-ruthenium oxide composite nanofiber material shows a trend of first increasing and then decreasing, and the best photocatalytic activity is exhibited when the mass of ruthenium trichloride is 0.5% of the theoretical mass of titanium dioxide. The photocatalytic hydrogen production activity of titanium dioxide-ruthenium oxide composite nanofibers is significantly higher than that of single titanium dioxide nanofibers. It can be seen that the in-situ growth of ruthenium oxide to modify titanium dioxide has a significant effect on improving its photocatalytic activity. Fig.10 The figure shows the results of the hydrogen production performance comparison of Examples 9 to 16 and Comparative Examples 3 to 4. As can be seen from the figure, the titanium dioxide-ruthenium oxide composite nanofiber has hydrogen evolution performance in simulated seawater environments under different conditions.

[0144] For matters not mentioned above, the prior art applies.

[0145] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are only for illustration, not for limiting the scope of the present invention, and those skilled in the art of the present invention can make various modifications or supplements to the described specific embodiments or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modification, equivalent substitution, improvement, etc. made to the above implementation modes according to the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium dioxide-ruthenium oxide composite nanofiber material for hydrogen production from seawater, characterized in that: The titanium dioxide-ruthenium oxide composite nanofiber material is prepared by an electrostatic spinning method and a calcination method, and comprises the following specific steps: S1. Preparation of nanofiber precursor: uniformly mix titanium source with ethanol and acetic acid, add spinning aid and ruthenium source, stir and mix to obtain a mixed solution, and obtain nanofiber precursor by electrospinning the mixed solution; the amount of ruthenium source added is 0.2%~3% of the mass of the titanium source; the distance between the spinning needle and the receiving plate is maintained at 10~20 cm, the voltage is 10~20 kV, and the spinning rate is 1.0~3.0 mL / h; The mass ratio of the titanium source, ethanol and acetic acid is 1:4:1 to 1:6:1; The ruthenium source is any one of ruthenium carbonate, ruthenium chloride, ruthenium acetate, ruthenium sulfate and ammonium hexachlororuthenate; The titanium source is any one of tetrabutyl titanate, isopropyl titanate and tetraethyl titanate; The spinning aid is any one of polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol and polyglycolic acid; S2, calcination treatment: calcining the nanofiber precursor solution prepared in step S1 under air atmosphere to obtain titanium dioxide-ruthenium oxide composite nanofibers; The calcination process is to continuously increase the temperature to 400~600℃ at a heating rate of 1~3℃ / min and maintain it for 2~4h.

2. A titanium dioxide-ruthenium oxide composite nanofiber material for hydrogen production from seawater, characterized in that: The method is prepared according to claim 1.

3. The titanium dioxide-ruthenium oxide composite nanofiber material according to claim 2, characterized in that: The diameter of the titanium dioxide-ruthenium oxide composite nanofiber material is 100-200 nm.

4. A method for producing hydrogen using seawater, characterized in that: A xenon lamp is used as a light source and the titanium dioxide-ruthenium oxide composite nanofiber material as described in any one of claims 2 to 3 is used to reduce H2O in seawater into H2.