A kind of anti-pollution porcelain insulator for DC ultra-high voltage transmission line and its preparation method
By forming an anti-fouling coating with a dense fine-grained structure on the surface of the insulator, combined with photocatalytic performance, the problem of pollution flashover of insulators in ultra-high voltage DC transmission lines is solved, and excellent anti-fouling performance and anti-fouling flashover effects are achieved.
Patent Information
- Application Number
- CN202310573395.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-05-22
AI Technical Summary
In ultra-high voltage DC transmission lines, insulator pollution flashover accidents occur frequently, resulting in economic losses and social impacts. It is difficult to effectively prevent contamination from firmly adhering to and removing from the surface with existing technology.
Nano-alumina, transition metal oxides, low-melting-point metals, burning aids, graphene-molybdenum disulfide nanocomposites and titanium dioxide sol are used as antifouling coatings, and dense fine grains are formed on the surface of the alumina matrix through ball milling and sintering processes. structure, combined with photocatalytic performance, improves the anti-fouling performance of insulators.
The insulator has achieved excellent anti-fouling performance and good anti-fouling flashover performance. Through the combination of rare earth-doped modified titanium dioxide and graphene-molybdenum disulfide nanocomposite, the recombination rate of photogenerated electrons is slowed down, the photocatalytic activity is improved, and the coating is ensured. The strong combination between the layer and the matrix enhances the resistance to contamination.
Smart Images

Figure BDA0004239246310000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of insulators, and specifically to an anti-pollution porcelain insulator for a DC ultra-high voltage transmission line and a preparation method thereof. Background Art
[0002] High-voltage direct current transmission is a high-power long-distance direct current transmission that utilizes the advantages of stable direct current, such as no inductive reactance, no capacitive reactance, and no synchronization problems. Compared with AC transmission, the higher transmission voltage of direct current transmission makes the importance of external insulating equipment such as insulators more prominent. If pollution flashover occurs in insulators in ultra-high-voltage direct current transmission lines, it will cause great economic losses and social impacts.
[0003] Nano-titanium dioxide coating has photocatalytic properties under ultraviolet light. Therefore, by applying a layer of nano-titanium dioxide coating on the surface of porcelain insulators, the dirt attached to the surface of the insulator can be oxidized and decomposed by light and is not easy to adhere firmly to the surface. Under the action of external wind, water flushing or gravity, it will automatically peel off from the surface of the insulator, thereby improving the anti-pollution performance of the insulator. It is one of the effective ways to solve insulator pollution flashover accidents and is also one of the current research hotspots. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes an anti-pollution porcelain insulator for DC ultra-high voltage transmission lines and a preparation method thereof.
[0005] The technical solutions adopted are as follows:
[0006] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line comprises an alumina substrate and a surface coating; the raw materials for preparing the surface coating include:
[0007] Nano-alumina, transition metal oxides, low melting point metals, sintering aids, graphene-molybdenum disulfide nanocomposites, and titanium dioxide sol.
[0008] Furthermore, the raw materials for preparing the surface coating include, by weight:
[0009] 20-30 parts of nano-alumina, 5-10 parts of transition metal oxide, 0.5-1 parts of low melting point metal, 1-3 parts of sintering aid, 1-2 parts of graphene-molybdenum disulfide nanocomposite material, and 60-80 parts of titanium dioxide sol.
[0010] Furthermore, the transition metal oxide is any one or more of chromium oxide, manganese oxide, iron oxide, cobalt oxide, nickel oxide, copper oxide, zinc oxide, and scandium oxide. The transition metal oxide is preferably manganese oxide and scandium oxide, and the weight ratio of manganese oxide to scandium oxide is preferably 1-5:1-5.
[0011] Furthermore, the low melting point metal is any one or more of indium, lithium, and bismuth, preferably indium.
[0012] Furthermore, the sintering aid is Bi-B-Si lead-free glass powder.
[0013] Furthermore, the preparation method of the graphene-molybdenum disulfide nanocomposite material is as follows:
[0014] Add ammonium molybdate and sodium sulfide to the graphene oxide dispersion, and then add hydrazine hydrate after ultrasonic oscillation treatment. Heat to 160-180°C in a sealed manner for hydrothermal reaction for 24-48 hours. Return to room temperature and filter. Wash with ethanol and water and then dry.
[0015] Furthermore, the preparation method of the titanium dioxide sol is as follows:
[0016] Titanium alkoxide, acid and ethanol are mixed evenly to obtain a first solution, rare earth nitrate and dispersant are dissolved in water to obtain a second solution, the second solution is added to the first solution and mixed evenly, and aged at 30-40° C. for 30-60 minutes to obtain the titanium dioxide sol.
[0017] Specifically, titanium alkoxide refers to a class of compounds containing at least one Ti-OC bond in its molecular structure, selected from isopropyl titanate or tetrabutyl titanate;
[0018] Specifically, the acid is selected from nitric acid, sulfuric acid, hydrochloric acid, and acetic acid;
[0019] Furthermore, the rare earth nitrate is any one or more of lanthanum nitrate, cerium nitrate, samarium nitrate or europium nitrate, preferably europium nitrate.
[0020] The present invention also provides a method for preparing an anti-pollution porcelain insulator for a DC ultra-high voltage transmission line:
[0021] Under the protection of inert gas, nano-alumina, transition metal oxide, low melting point metal, sintering aid and graphene-molybdenum disulfide nanocomposite material are mixed and ball-milled and then added to titanium dioxide sol to obtain a mixed sol, and the mixed sol is coated on the surface of the alumina substrate by any one of pulling, brushing or spin coating, first vacuum dried at 50-80°C for 10 hours, then placed in an environment with an oxygen content greater than 21%, heated to 250-300°C within 10-20 minutes, kept warm for 1-4 hours, then heated to 1380-1420°C for sintering for 1-2 hours, cooled to room temperature, then heated to 480-500°C for keeping warm for 1-2 hours, and finally cooled to room temperature.
[0022] Furthermore, the ball milling adopts a planetary ball mill, the ball milling speed is 100-300r / min, and the ball milling time is greater than 10h.
[0023] The beneficial effects of the present invention are as follows: the transition metal oxide can hinder the growth of grains, promote the densification of the coating and the formation of a fine-grained structure, and can also form a glass phase with nano-alumina. During sintering, the glass phase with the same composition as that in the alumina matrix diffuses mutually, promoting the firm bonding between the surface coating and the alumina matrix. Indium can melt and penetrate between ceramic particles at a relatively low temperature, wets the surface well and improves the bonding performance. The indium oxide formed after oxidation and the transition metal oxide together improve the anti-pollution flashover performance of the insulator. The titanium dioxide with photocatalytic properties is doped and modified by rare earth, and then the graphene-molybdenum disulfide nanocomposite is introduced. The material makes it easier for the photogenerated electrons of titanium dioxide to transfer to the surface of the graphene-molybdenum disulfide nanocomposite material, slowing down the rate of recombination of photogenerated electrons and holes. If there is no graphene-molybdenum disulfide nanocomposite material, the photogenerated electrons of titanium dioxide will quickly recombine with holes, thereby reducing the photocatalytic activity. The present invention selects nano-alumina, transition metal oxides, low-melting point metals, sintering aids, graphene-molybdenum disulfide nanocomposite materials, and titanium dioxide sol as surface coating components of anti-pollution porcelain insulators. Through optimized combination, the finally prepared anti-pollution porcelain insulator has excellent anti-pollution performance and good anti-pollution flashover performance. DETAILED DESCRIPTION
[0024] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0025] Nano-alumina: Zhengzhou Jinzhong New Materials Technology Co., Ltd.;
[0026] Manganese oxide: Qinghe County Top Metal Materials Co., Ltd.;
[0027] Scandium oxide: Qinghe County Top Metal Materials Co., Ltd.;
[0028] Indium powder: Qinghe County Top Metal Materials Co., Ltd.
[0029] Bi-B-Si lead-free glass powder: PM-600, Xi'an Xinzheng Electronic Materials Co., Ltd.;
[0030] Graphene-MoS2 nanocomposite: homemade;
[0031] Titanium dioxide sol: homemade.
[0032] Embodiment 1:
[0033] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line, comprising an alumina substrate and a surface coating;
[0034] The raw materials for preparing the surface coating include, by weight:
[0035] 28 parts of nano-alumina, 2.5 parts of manganese oxide, 5 parts of scandium oxide, 1 part of indium powder, 2 parts of Bi-B-Si lead-free glass powder, 1.5 parts of graphene-molybdenum disulfide nanocomposite material, and 70 parts of titanium dioxide sol.
[0036] Wherein, the preparation method of graphene-molybdenum disulfide nanocomposite material is as follows:
[0037] Add 20g of ammonium molybdate and 20g of sodium sulfide to 500mL of graphene oxide dispersion (20mg / mL), treat with ultrasonic oscillation for 1h, transfer to a hydrothermal reactor, add 40mL of hydrazine hydrate, stir evenly, seal and heat to 175℃ for hydrothermal reaction for 24h, return to room temperature and filter, wash with ethanol and water 3 times each, and then vacuum dry to constant weight.
[0038] The preparation method of titanium dioxide sol is as follows:
[0039] 172.8 mL of tetrabutyl titanate, 30 mL of nitric acid, and 650 mL of ethanol were mixed evenly to obtain a first solution, 2.23 g of europium nitrate hexahydrate and dispersant polyethylene glycol 400 were dissolved in 100 mL of water to obtain a second solution, and the second solution was added dropwise to the first solution for 15 minutes. After the addition was completed, the mixture was mixed evenly and aged at 40° C. for 60 minutes to obtain a titanium dioxide sol.
[0040] The preparation method of the above-mentioned anti-pollution porcelain insulator for DC ultra-high voltage transmission line:
[0041] Under argon protection, nano-alumina, manganese oxide, scandium oxide, indium powder, Bi-B-Si lead-free glass powder, and graphene-molybdenum disulfide nanocomposite materials were mixed and ball-milled using a planetary ball mill with a ball milling speed of 150 r / min and ethanol as the ball milling medium for 12 h. After ball milling, the mixture was dried and added to titanium dioxide sol to obtain a mixed sol. The mixed sol was coated on the surface of the alumina substrate using a Czochralski method, and then placed in a vacuum drying oven at 60°C for 10 h, and then placed in an environment of 1:1 oxygen and nitrogen for heating. The mixture was first heated to 280°C within 15 min, kept warm for 2 h, then heated to 1400°C for sintering for 2 h, cooled to room temperature, and then heated to 480°C for 1 h, and finally cooled to room temperature.
[0042] Embodiment 2:
[0043] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line, comprising an alumina substrate and a surface coating;
[0044] The raw materials for preparing the surface coating include, by weight:
[0045] 30 parts of nano-alumina, 5 parts of manganese oxide, 5 parts of scandium oxide, 1 part of indium powder, 3 parts of Bi-B-Si lead-free glass powder, 2 parts of graphene-molybdenum disulfide nanocomposite material, and 80 parts of titanium dioxide sol.
[0046] Wherein, the preparation method of graphene-molybdenum disulfide nanocomposite material and titanium dioxide sol is the same as that in Example 1.
[0047] The preparation method of the above-mentioned anti-pollution porcelain insulator for DC ultra-high voltage transmission line:
[0048] Under argon protection, nano-alumina, manganese oxide, scandium oxide, indium powder, Bi-B-Si lead-free glass powder, and graphene-molybdenum disulfide nanocomposite materials were mixed and ball-milled using a planetary ball mill with a ball milling speed of 150 r / min and ethanol as the ball milling medium for 12 h. After ball milling, the mixture was dried and added to titanium dioxide sol to obtain a mixed sol. The mixed sol was coated on the surface of the alumina substrate using a Czochralski method, and then placed in a vacuum drying oven at 80°C for 10 h, and then placed in an environment of 1:1 oxygen and nitrogen for heating. The mixture was first heated to 300°C within 20 min, kept warm for 4 h, then heated to 1420°C for sintering for 2 h, cooled to room temperature, and then heated to 500°C for 2 h, and finally cooled to room temperature.
[0049] Embodiment 3:
[0050] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line, comprising an alumina substrate and a surface coating;
[0051] The raw materials for preparing the surface coating include, by weight:
[0052] 20 parts of nano-alumina, 2.5 parts of manganese oxide, 2.5 parts of scandium oxide, 0.5 parts of indium powder, 1 part of Bi-B-Si lead-free glass powder, 1 part of graphene-molybdenum disulfide nanocomposite material, and 60 parts of titanium dioxide sol.
[0053] Wherein, the preparation method of graphene-molybdenum disulfide nanocomposite material and titanium dioxide sol is the same as that in Example 1.
[0054] The preparation method of the above-mentioned anti-pollution porcelain insulator for DC ultra-high voltage transmission line:
[0055] Under argon protection, nano-alumina, manganese oxide, scandium oxide, indium powder, Bi-B-Si lead-free glass powder, and graphene-molybdenum disulfide nanocomposite materials were mixed and ball-milled using a planetary ball mill with a ball milling speed of 150 r / min and ethanol as the ball milling medium for 12 h. After ball milling, the mixture was dried and added to titanium dioxide sol to obtain a mixed sol. The mixed sol was coated on the surface of the alumina substrate using a Czochralski method, and then placed in a vacuum drying oven at 50°C for 10 h, and then placed in an environment of 1:1 oxygen and nitrogen for heating. The mixture was first heated to 250°C within 10 min, kept warm for 1 h, then heated to 1380°C for sintering for 1 h, cooled to room temperature, then heated to 480°C for 1 h, and finally cooled to room temperature.
[0056] Embodiment 4:
[0057] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line, comprising an alumina substrate and a surface coating;
[0058] The raw materials for preparing the surface coating include, by weight:
[0059] 30 parts of nano-alumina, 2.5 parts of manganese oxide, 5 parts of scandium oxide, 0.5 parts of indium powder, 3 parts of Bi-B-Si lead-free glass powder, 1 part of graphene-molybdenum disulfide nanocomposite material, and 80 parts of titanium dioxide sol.
[0060] Wherein, the preparation method of graphene-molybdenum disulfide nanocomposite material and titanium dioxide sol is the same as that in Example 1.
[0061] The preparation method of the above-mentioned anti-pollution porcelain insulator for DC ultra-high voltage transmission line:
[0062] Under argon protection, nano-alumina, manganese oxide, scandium oxide, indium powder, Bi-B-Si lead-free glass powder, and graphene-molybdenum disulfide nanocomposite materials were mixed and ball-milled using a planetary ball mill with a ball milling speed of 150 r / min and ethanol as the ball milling medium for 12 h. After ball milling, the mixture was dried and added to titanium dioxide sol to obtain a mixed sol. The mixed sol was coated on the surface of the alumina substrate using a Czochralski method, and then placed in a vacuum drying oven at 50°C for 10 h, and then placed in an environment of 1:1 oxygen and nitrogen for heating. The mixture was first heated to 250°C within 20 min, kept warm for 4 h, then heated to 1380°C for sintering for 2 h, cooled to room temperature, and then heated to 480°C for 2 h, and finally cooled to room temperature.
[0063] Embodiment 5:
[0064] An anti-pollution porcelain insulator for a DC ultra-high voltage transmission line, comprising an alumina substrate and a surface coating;
[0065] The raw materials for preparing the surface coating include, by weight:
[0066] 20 parts of nano-alumina, 5 parts of manganese oxide, 2.5 parts of scandium oxide, 1 part of indium powder, 1 part of Bi-B-Si lead-free glass powder, 2 parts of graphene-molybdenum disulfide nanocomposite material, and 60 parts of titanium dioxide sol.
[0067] Wherein, the preparation method of graphene-molybdenum disulfide nanocomposite material and titanium dioxide sol is the same as that in Example 1.
[0068] The preparation method of the above-mentioned anti-pollution porcelain insulator for DC ultra-high voltage transmission line:
[0069] Under argon protection, nano-alumina, manganese oxide, scandium oxide, indium powder, Bi-B-Si lead-free glass powder, and graphene-molybdenum disulfide nanocomposite materials were mixed and ball-milled using a planetary ball mill with a ball milling speed of 150 r / min and ethanol as the ball milling medium for 12 h. After ball milling, the mixture was dried and added to titanium dioxide sol to obtain a mixed sol. The mixed sol was coated on the surface of the alumina substrate using a Czochralski method, and then placed in a vacuum drying oven at 80°C for 10 h, and then placed in an environment of 1:1 oxygen and nitrogen for heating. The mixture was first heated to 300°C within 10 min, kept warm for 1 h, then heated to 1420°C for sintering for 1 h, cooled to room temperature, and then heated to 500°C for 1 h, and finally cooled to room temperature.
[0070] Comparative Example 1:
[0071] The method is basically the same as Example 1, except that no indium powder is added.
[0072] Comparative Example 2:
[0073] The method is basically the same as Example 1, except that an equal weight of commercially available indium oxide is used to replace the indium powder.
[0074] Comparative Example 3:
[0075] The method is basically the same as Example 1, except that manganese oxide and scandium oxide are not added.
[0076] Comparative Example 4:
[0077] The method is basically the same as Example 1, except that the graphene-molybdenum disulfide nanocomposite material is not added.
[0078] Comparative Example 5:
[0079] The method is substantially the same as Example 1, except that an equal weight of commercially available graphene is used to replace the graphene-molybdenum disulfide nanocomposite material.
[0080] Comparative Example 6:
[0081] The method is basically the same as Example 1, except that europium nitrate hexahydrate is not added during the preparation of the titanium dioxide sol.
[0082] Performance Test:
[0083] The anti-pollution porcelain insulators prepared in Examples 1-5 and Comparative Examples 1-6 were taken as samples for performance testing;
[0084] ① The samples were added into 100mL methyl orange solution (40mg / L) for photocatalytic degradation experiment. The visible light intensity at the surface of the solution was 10mW / cm 2 During the degradation process, samples were taken every 30 minutes, and 5 mL was sampled each time. The absorbance was measured by TU-1901 UV-visible spectrophotometer to analyze the change of methyl orange concentration. The photocatalytic degradation rate was then calculated based on the change in absorbance. The 2h photocatalytic degradation rate is shown in Table 1.
[0085] ② Use ball milling method to mix sodium chloride and diatomaceous earth with a particle size of 2000 mesh at a mass ratio of 1:5, and put them in a 120℃ oven for drying for 30 minutes before accumulation of dirt to remove the moisture absorbed from the air to obtain the dirt. Weigh the sample mass, place the sample in an artificial dirt accumulation box, start the high-voltage power supply, make the sample in an electric field with a field strength of 0.7kV / cm, start the air compressor to form negative pressure, suck the dirt into the artificial dirt accumulation box, blow it out in a mist, and settle naturally. Each time the dirt accumulates, the mass of the dirt is 12g. Each sample accumulates dirt 5 times. After turning off the high-voltage power supply, take out the sample, wipe off the dirt on the edge and back of the sample, weigh the sample mass, and the mass difference before and after the sample is the amount of dirt accumulation;
[0086] ③ Use ball milling method to mix sodium chloride, diatomaceous earth with particle size of 2000 mesh, and water in a mass ratio of 1:5:15. Use quantitative brushing method to evenly smear the samples, and then wet the samples in the artificial ultrasonic fog test box built in the laboratory. The water used in the test is deionized water with a conductivity of 12.68μS / cm. The test power supply is 600kV / 0.5A thyristor double feedback double voltage rectifier DC test power supply. When the leakage current is 0.5A, its dynamic voltage drop is less than 5%, and the ripple factor of the voltage during flashover is less than 3%, which meets the IEC standard and national standard and the power supply requirements for DC pollution test. The electrode uses a cylindrical electrode. The test steps are as follows: Place the smeared sample horizontally in the artificial ultrasonic fog test box, turn on the ultrasonic fog generator, and use 15.86mL / (m 3·min) of atomization volume is continuously supplied, the high-voltage power supply is turned on, and a 200 kV DC voltage is applied between the two circular electrodes, that is, wetting under a DC electric field, for 10 min, and the voltage is increased at a uniform rate of 5 kV / s until flashover occurs on the surface of the sample, and the flashover voltage, that is, the highest voltage value occurring during the pressurization process, is recorded. After repeating the test 3 times for each sample, the average value is taken. The results are shown in Table 1;
[0087] Table 1:
[0088]
[0089] It can be seen from Table 1 above that the anti-pollution porcelain insulator prepared by the present invention has excellent anti-pollution performance and good anti-pollution flashover performance.
[0090] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An anti-pollution porcelain insulator for DC ultra-high voltage transmission lines, characterized in that: including an alumina substrate and a surface coating; The raw materials for preparing the surface coating include, by weight: 20-30 parts of nano-alumina, 5-10 parts of transition metal oxide, 0.5-1 parts of low melting point metal, 1-3 parts of sintering aid, 1-2 parts of graphene-molybdenum disulfide nanocomposite material, 60-80 parts of titanium dioxide sol; The transition metal oxide is manganese oxide and scandium oxide, and the weight ratio of manganese oxide to scandium oxide is 1-5:1-5; The low melting point metal is indium; The sintering aid is Bi-B-Si lead-free glass powder; The preparation method of the graphene-molybdenum disulfide nanocomposite material is as follows: Add ammonium molybdate and sodium sulfide to the graphene oxide dispersion, treat with ultrasonic vibration, then add hydrazine hydrate, heat to 160-180°C for hydrothermal reaction for 24-48h, return to room temperature and filter, wash with ethanol and water and dry; The preparation method of the titanium dioxide sol is as follows: Titanium alkoxide, acid and ethanol are mixed uniformly to obtain a first solution, rare earth nitrate and dispersant are dissolved in water to obtain a second solution, the second solution is added to the first solution and mixed uniformly, and aged at 30-40° C. for 30-60 minutes to obtain the titanium dioxide sol; The rare earth nitrate is europium nitrate; The preparation method of the anti-pollution porcelain insulator for DC ultra-high voltage transmission line: Under the protection of inert gas, nano-alumina, transition metal oxide, low melting point metal, sintering aid and graphene-molybdenum disulfide nanocomposite material are mixed and ball-milled and then added to titanium dioxide sol to obtain a mixed sol, and the mixed sol is coated on the surface of the alumina substrate by any one of pulling, brushing or spin coating, first vacuum dried at 50-80°C for 10 hours, then placed in an environment with an oxygen content greater than 21%, heated to 250-300°C within 10-20 minutes, kept warm for 1-4 hours, then heated to 1380-1420°C for sintering for 1-2 hours, cooled to room temperature, then heated to 480-500°C for keeping warm for 1-2 hours, and finally cooled to room temperature.
2. A method for preparing an anti-pollution porcelain insulator for a DC ultra-high voltage transmission line according to claim 1, characterized in that: Under the protection of inert gas, nano-alumina, transition metal oxide, low melting point metal, sintering aid and graphene-molybdenum disulfide nanocomposite material are mixed and ball-milled and then added to titanium dioxide sol to obtain a mixed sol, and the mixed sol is coated on the surface of the alumina substrate by any one of pulling, brushing or spin coating, first vacuum dried at 50-80°C for 10 hours, then placed in an environment with an oxygen content greater than 21%, heated to 250-300°C within 10-20 minutes, kept warm for 1-4 hours, then heated to 1380-1420°C for sintering for 1-2 hours, cooled to room temperature, then heated to 480-500°C for keeping warm for 1-2 hours, and finally cooled to room temperature.
3. The method for preparing anti-pollution porcelain insulator for DC ultra-high voltage transmission line according to claim 2, characterized in that: The ball milling adopts a planetary ball mill, the ball milling speed is 100-300r / min, and the ball milling time is greater than 10h.