A corrosion inhibitor and preparation method thereof

By preparing a corrosion inhibitor containing ether bonds, quaternary ammonium groups and hydrophobic groups in oil well development, the problem of insufficient corrosion inhibition in high-temperature, high-salt, and high-sulfur environments was solved, achieving efficient metal protection and maximum corrosion inhibition. The rate can reach more than 95%.

CN116640564BActive Publication Date: 2024-10-15XINJIANG LIKE PETROCHEMICAL TECH SERVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310623706.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-10-15
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

In the development process of oil wells with high temperature, high salt and high sulfur content, conventional corrosion inhibitors show insufficient corrosion inhibition effect in high temperature, high salt and high sulfur content environments, resulting in serious oil casing corrosion problems.

Method used

A corrosion inhibitor prepared through a two-step reaction, using materials such as p-hydroxybenzaldehyde, 1,2-dibromoethane, tertiary amines and small molecule ether amines to generate products containing ether bonds, quaternary ammonium groups and hydrophobic groups , enhance its adsorption performance on metal surfaces, thereby slowing down corrosion.

Benefits of technology

Under the conditions of salinity of 50,000, hydrogen sulfide equivalent content of about 0.12g/L, and temperature of 90°C, the maximum corrosion inhibition effect can reach more than 95%, and the dosage is only 200ppm, which is significant. Improved metal protection effect in high temperature, high salt and high sulfur environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004256216830000021
    Figure BDA0004256216830000021
  • Figure BDA0004256216830000051
    Figure BDA0004256216830000051
  • Figure BDA0004256216830000061
    Figure BDA0004256216830000061
Patent Text Reader

Abstract

The present invention provides a corrosion inhibitor and a preparation method thereof, and relates to the technical field of oilfield additives. The preparation method of the corrosion inhibitor comprises the following steps: taking p-hydroxybenzaldehyde and dissolving it in a first solvent, adding 1,2-dibromoethane and an acid binding agent, reacting at 60-80°C for 10-24h, and after the reaction is completed, separating and purifying it to obtain a first monomer, wherein the molar amount of 1,2-dibromoethane is greater than the molar amount of p-hydroxybenzaldehyde; taking the first monomer and a tertiary amine, adding them to ethanol, reacting at 50-80°C for 1-3h, adding a small molecule ether amine after the reaction is completed, and continuing to react for 2-5h, after the reaction is completed, removing ethanol to obtain. The corrosion inhibitor of the present invention has relatively mild preparation conditions, does not involve high temperature and pressure links, and its preparation method is relatively simple. The prepared corrosion inhibitor has a good corrosion inhibition effect. Under the conditions of a mineralization degree of 50,000, an equivalent hydrogen sulfide content of about 0.12 g / L, and a temperature of 90°C, its maximum corrosion inhibition effect can reach more than 95%, and its added dosage is only 200 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil field additives, and particularly relates to a corrosion inhibitor for oil and gas wells and a preparation method thereof. Background Art

[0002] With the corrosion in the process of oil and gas field exploitation in my country, the failure problems such as corrosion and perforation of oil casing can no longer be ignored. Especially in recent years, the continuous development of acidic oil and gas fields has made oil well equipment face more and more serious corrosion problems. In the process of oil well development, its corrosion is usually due to the presence of a large amount of inorganic salts in the produced fluid. At the same time, in some environments, it will also carry some hydrogen sulfide gas. These inorganic salts and hydrogen sulfide are important factors affecting metal corrosion. At present, for some highly corrosive environments, such as high-temperature, high-salt and high-sulfur oil reservoirs, the composition of conventional corrosion inhibitors, especially compound corrosion inhibitors, will change, and even some components will precipitate, resulting in relatively insufficient corrosion inhibition effect in the environment of high-temperature, high-salt and high-sulfur oil reservoirs. Summary of the invention

[0003] In order to solve at least one of the above problems, the present invention proposes a method for preparing a corrosion inhibitor. The method is simple, and the prepared corrosion inhibitor can be applied to a high-temperature, high-salt, and high-sulfur environment.

[0004] The technical solution of the present invention is as follows: A method for preparing a corrosion inhibitor comprises the following steps:

[0005] S1, dissolving p-hydroxybenzaldehyde in a first solvent, adding 1,2-dibromoethane and an acid binding agent, reacting at 60-80° C. for 10-24 hours, and after the reaction is completed, separating and purifying the first monomer, wherein the molar amount of 1,2-dibromoethane is greater than the molar amount of p-hydroxybenzaldehyde;

[0006] S2. Take the first monomer and the tertiary amine, add them to ethanol, react at 50-80°C for 1-3h, add a small molecule ether amine after the reaction, continue to react for 2-5h, remove the ethanol after the reaction, wherein the molar ratio of the first monomer, the tertiary amine and the small molecule ether amine is 1:0.6-1.0:1-1.5; the small molecule ether amine refers to an ether amine with a molecular weight of less than 150, containing one primary amine and at least one ether bond; the molecular formula of the tertiary amine is as follows:

[0007] wherein R1, R2, and R3 are independently one of CH3, CH3CH2, CH3CH2CH2 or HOCH2CH2.

[0008] Specifically, in the present invention, the purpose of S1 is to prepare a first monomer containing a benzene ring, an aldehyde group, an ether bond and a halogen atom at the same time. Therefore, in this process, the reaction equation is as follows:

[0009]

[0010] The purpose of adding an acid binder is to make the reaction proceed to the right and increase the yield.

[0011] After obtaining the first monomer, the first monomer is reacted with a tertiary amine. Since the first monomer contains corresponding halogen atoms, the first monomer can undergo a quaternization reaction with the tertiary amine to generate a quaternary ammonium salt. The generated quaternary ammonium salt can be adsorbed on the metal surface to achieve a corrosion inhibition effect. At the same time, the molar ratio of the first monomer to the tertiary amine is limited to 1:0.6-1.0 in order to facilitate subsequent reactions.

[0012] After the first monomer reacts with the tertiary amine, a small molecule ether amine is added. Since the small molecule ether amine contains a primary amine group, the primary amine group can react with the halogen atom that has not reacted completely in the previous step, and can also react with the aldehyde group to undergo a Schiff base reaction. The imine group generated by the Schiff base reaction can also be adsorbed on the metal surface to form a protective film to achieve a corrosion inhibition effect. At the same time, after the small molecule ether amine reacts with the alkyl halide, secondary amines and tertiary amines can also be generated (the reaction products are relatively complex).

[0013] The above-mentioned synthesized product contains ether bonds, quaternary ammonium groups and imino groups at the same time. Through the synergistic effect of multiple groups, the adsorption performance of the product on the metal surface can be increased; at the same time, the above-mentioned product also includes hydrophobic groups such as alkyl groups and benzene rings. When the product is adsorbed on the metal surface, the hydrophobic groups will hinder water from further contacting the metal surface, thereby increasing its corrosion inhibition effect.

[0014] Meanwhile, in S2, the reason why only the solvent needs to be simply removed is that some unreacted raw materials, such as etheramine and tertiary amine, are shale inhibitors and will not affect the fluid in the well.

[0015] In one embodiment of the present invention, the first solvent is one of ethanol, propanol or isopropanol, and ethanol is preferred in terms of availability.

[0016] One embodiment of the present invention is that the acid binding agent is one of sodium carbonate and potassium carbonate, and the amount of the acid binding agent added is greater than the molar amount of the p-hydroxybenzaldehyde. The function of the acid binding agent is to absorb the acid generated during the reaction so that the reaction proceeds to the right. Therefore, for the acid binding agent, a base is usually selected. From the perspective of cost and subsequent removal difficulty, a base that is poorly soluble or insoluble in the first solvent is preferred.

[0017] One embodiment of the present invention is that in S1, the separation and purification step is specifically as follows: filtering the product after the reaction, taking the filtrate, adding an organic solvent and a sodium hydroxide aqueous solution with a concentration of 1 to 3 mol / L, mixing, taking the organic layer, washing with saturated sodium chloride until neutral, and removing the solvent. In fact, the aqueous solution here can be a strong base such as potassium hydroxide or sodium hydroxide, but considering the cost problem, sodium hydroxide is used. Here, ethyl acetate is usually selected as the organic solvent. At the same time, in this process, after filtering the product, the first solvent can be removed to avoid its excessive volume and affect the subsequent extraction process.

[0018] One embodiment of the present invention is that in S1, the molar amount of the 1,2-dibromoethane is 3 to 5 times the molar amount of the p-hydroxybenzaldehyde.

[0019] An embodiment of the present invention is that the small molecule ether amine is one of 2-methoxyethylamine, 2-ethoxyethylamine, 3-methoxypropylamine and 3-ethoxypropylamine.

[0020] One embodiment of the present invention is that the molar ratio of the first monomer, the tertiary amine and the small molecule ether amine is 1:0.7-0.8:1.1-1.2. In this case, the prepared corrosion inhibitor has a better effect.

[0021] A corrosion inhibitor is prepared by any of the above methods, which can effectively reduce the corrosion of metals by produced water with high temperature, high salt and high hydrogen sulfide.

[0022] The beneficial effects of the present invention are:

[0023] The corrosion inhibitor of the present invention is prepared by a two-step reaction, and its preparation conditions are relatively mild, and it does not involve high temperature and pressure links. At the same time, its preparation method is relatively simple. The prepared corrosion inhibitor has a good corrosion inhibition effect. Under the conditions of a mineralization degree of 50,000, a hydrogen sulfide equivalent content of about 0.12 g / L, and a temperature of 90°C, its maximum corrosion inhibition effect can reach more than 95%, and its addition amount is only 200 ppm. DETAILED DESCRIPTION

[0024] In order to make the technical solutions and technical advantages of the present invention more clear, the technical solutions in the implementation process of the present invention will be clearly and completely described below in conjunction with embodiments.

[0025] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0026] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0027] Example 1

[0028] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 94 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and the mixture was shaken well, and then the ethyl acetate layer was separated after a period of time. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0029] Take 11.5g of the first monomer and 3.7g of N,N-dimethylpropylamine and add them to 200ml of ethanol. Reflux and react at 70°C for 2h. After the reaction, add 6.4g of 3-ethoxypropylamine and continue to react under the above conditions for 4h. After the reaction, remove the ethanol by vacuum distillation to obtain the product.

[0030] Example 2

[0031] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 25 g of 1,2-dibromoethane and 15 g of potassium carbonate were added, and the mixture was refluxed at 70° C. for 20 h. After the reaction, the product was filtered, and the filtrate was taken. A portion of the ethanol was evaporated, and 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added at the same time. After shaking, the mixture was waited for a while and the ethyl acetate layer was separated. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0032] Take 11.5g of the first monomer and 3.0g of N,N-dimethylpropylamine and add them to 200ml of ethanol. Reflux and react at 70°C for 2h. After the reaction, add 7.2g of 3-ethoxypropylamine and continue to react under the above conditions for 4h. After the reaction, remove the ethanol by vacuum distillation to obtain the product.

[0033] Example 3

[0034] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 94 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and the mixture was shaken well, and then the ethyl acetate layer was separated after a period of time. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0035] Take 11.5g of the first monomer and 3.7g of N,N-diethylpropylamine and add them to 200ml of ethanol. Reflux and react at 70°C for 3h. After the reaction, add 5.2g of 2-methoxyethylamine and continue to react under the above conditions for 4h. After the reaction, remove the ethanol by vacuum distillation.

[0036] Example 4

[0037] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 94 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and the mixture was shaken well, and then the ethyl acetate layer was separated after a period of time. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0038] Take 11.5g of the first monomer and 3.3g of N,N-dimethylethanolamine and add them to ethanol. Reflux at 70°C for 2h. After the reaction, add 5.9g of 3-ethoxypropylamine and continue to react under the above conditions for 4h. After the reaction, remove ethanol by vacuum distillation to obtain the product.

[0039] Comparative Example 1

[0040] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 18 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and the mixture was shaken well, and then the ethyl acetate layer was separated after a period of time. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0041] Take 11.5g of the first monomer and 3.5g of N,N-dimethylpropylamine and add them to 200ml of ethanol. Reflux and react at 70°C for 2h. After the reaction, add 6.7g of 3-ethoxypropylamine and continue to react under the above conditions for 4h. After the reaction, remove the ethanol by vacuum distillation to obtain the product.

[0042] Comparative Example 2

[0043] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 94 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and the mixture was shaken well, and then the ethyl acetate layer was separated after a period of time. The ethyl acetate layer was washed with saturated sodium chloride until it was neutral, and then the ethyl acetate was removed to obtain the first monomer;

[0044] 11.5 g of the first monomer and 3.7 g of N,N-dimethylpropylamine were added to 200 ml of ethanol, and refluxed at 70° C. for 2 h. After the reaction was completed, the ethanol was removed by vacuum distillation to obtain the product.

[0045] Comparative Example 3

[0046] 12.2 g of p-hydroxybenzaldehyde was added to 120 ml of ethanol, stirred to dissolve, and then 94 g of 1,2-dibromoethane and 12 g of sodium carbonate were added, and refluxed at 70° C. for 15 h. After the reaction was completed, the product was filtered, and the filtrate was taken, and a portion of the ethanol was evaporated. At the same time, 200 ml of a 2 mol / L sodium hydroxide aqueous solution and 200 ml of ethyl acetate were added, and after shaking, the mixture was waited for a while and the ethyl acetate layer was separated, and then the ethyl acetate was removed to obtain the first monomer;

[0047] 11.5 g of the first monomer and 6.4 g of 3-ethoxypropylamine were added to 200 ml of ethanol, and refluxed at 70° C. for 2 h. After the reaction was completed, the ethanol was removed by vacuum distillation to obtain the product.

[0048] In order to further illustrate the effect of the corrosion inhibitor for oil and gas wells prepared in the above embodiment, the corrosion inhibitor for oil and gas wells prepared above is tested below.

[0049] The dynamic uniform corrosion inhibition rate measurement method in the standard "SY / T5273-2014 Performance Indicators and Evaluation Methods of Corrosion Inhibitors for Oilfield Produced Water" was adopted, and an N80 steel hanging plate was used; the total salt content of the test liquid was 50 g / L, of which the sodium chloride concentration was 40 g / L, the calcium chloride concentration was 9.7 g / L, the sodium sulfide concentration was 0.3 g / L (equivalent to a hydrogen sulfide concentration of about 0.12 g / L), and its pH was about 4.5; at 90°C, the corrosion inhibitors prepared in the above embodiments and comparative examples were tested, and the final test results are shown in Table 1.

[0050] Table 1 Corrosion inhibition test results

[0051]

[0052]

[0053] As can be seen from Table 1, the corrosion inhibitor prepared in the embodiment of the present invention can be well applied to corrosion inhibition under high temperature, high salt and hydrogen sulfide conditions. When the addition amount is 50ppm, the maximum corrosion inhibition rate can reach 92.3%; when the addition amount is 20ppm, the maximum corrosion inhibition rate can reach 95.7%.

[0054] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a corrosion inhibitor, characterized in that: The following steps are involved: S1, dissolving p-hydroxybenzaldehyde in a first solvent, adding 1,2-dibromoethane and an acid binding agent, reacting at 60-80° C. for 10-24 hours, and after the reaction is completed, separating and purifying the first monomer, wherein the molar amount of 1,2-dibromoethane is greater than the molar amount of p-hydroxybenzaldehyde; S2. Take the first monomer and the tertiary amine, add them to ethanol, react at 50-80°C for 1-3h, add a small molecule ether amine after the reaction, continue to react for 2-5h, remove the ethanol after the reaction, wherein the molar ratio of the first monomer, the tertiary amine and the small molecule ether amine is 1:0.6-1.0:1-1.5; the molecular formula of the tertiary amine is as follows: , wherein R1, R2, and R3 are independently one of CH3, CH3CH2, CH3CH2CH2, or HOCH2CH2; the small molecule ether amine is one of 2-methoxyethylamine, 2-ethoxyethylamine, 3-methoxypropylamine, and 3-ethoxypropylamine; The amount of the acid binding agent added is greater than the molar amount of the p-hydroxybenzaldehyde.

2. The method according to claim 1, characterized in that The first solvent is one of ethanol, propanol or isopropanol.

3. The method according to claim 1, characterized in that The acid binding agent is one of sodium carbonate and potassium carbonate.

4. The method according to claim 1, characterized in that In S1, the separation and purification step is specifically as follows: filtering the product after the reaction, adding an organic solvent and a sodium hydroxide aqueous solution with a concentration of 1 to 3 mol / L to the filtrate, mixing, taking the organic layer, washing with saturated sodium chloride until neutral, and removing the solvent to obtain.

5. The method according to claim 1, characterized in that In S1, the molar amount of the 1,2-dibromoethane is 3 to 5 times the molar amount of the p-hydroxybenzaldehyde.

6. The method according to claim 1, characterized in that The molar ratio of the first monomer, the tertiary amine and the small molecule ether amine is 1:0.7-0.8:1.1-1.

2.

7. A corrosion inhibitor prepared by the method according to any one of claims 1 to 6.