Preparation method of Al2O3 dispersion strengthened copper alloy material

By combining mechanical alloying method and internal oxidation method, mixed grinding, internal oxidation and H2 deoxygenation processes are adopted to solve the problems of long production cycle, high cost and pollution in the preparation of Al2O3 diffusion reinforced copper alloy materials, and the production cycle is shortened and the cost is achieved. Reduce and refine particles to adapt to the effect of industrial mass production.

CN116640955BActive Publication Date: 2024-11-19XINJIANG HESHENG INNOVATIVE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310625979.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-11-19
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The existing preparation process of Al2O3 diffusion reinforced copper alloy materials has problems such as long production cycle, high cost, large Al2O3 particles, difficulty in adapting to industrial mass production and easy pollution.

Method used

The Al2O3 diffusion-strengthening copper alloy material was prepared by combining mechanical alloying method and internal oxidation method. The specific steps include mixing copper powder, aluminum powder and CuO powder and ball milling, followed by sintering and reducing treatment in a vacuum sintering furnace and hydrogen atmosphere, and finally pressing and forming.

Benefits of technology

It greatly shortens the production cycle and reduces production costs. The obtained Al2O3 particles are smaller, reduces impurities, adapts to industrial mass production, and maintains the high temperature strength of the material and clean crystal surface.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of dispersion-strengthened copper-based composite materials, and is a method for preparing an Al2O3 dispersion-strengthened copper alloy material; the method is carried out according to the following steps: the first step is to mix copper powder, aluminum powder and CuO powder, add stearic acid, and ball-mill to obtain primary alloy powder; the second step is sintering treatment; the third step is to add stearic acid and mix after crushing, and ball-mill to obtain secondary alloy powder; the fourth step is to reduce excess oxygen in a hydrogen atmosphere; the fifth step is to press and form and sinter again to obtain an Al2O3 dispersion-strengthened copper alloy material. The invention combines mechanical alloying method with internal oxidation method for the first time, and obtains Al2O3 dispersion-strengthened copper alloy material through mixed grinding, internal oxidation of mixed powder, secondary grinding, H2 removal of excess oxygen and pressing and sintering processes; the invention greatly shortens the production cycle compared with the existing process, has low production cost, less impurities, smaller Al2O3 particles, and is more adaptable to industrial mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dispersion-strengthened copper-based composite materials, in particular to a method for preparing an Al2O3 dispersion-strengthened copper alloy material. Background Art

[0002] Al2O3 dispersion-strengthened copper alloy is a new type of composite material with excellent comprehensive physical and mechanical properties. It has high strength, high conductivity and good resistance to high temperature softening. It is widely used in the fields of electronics, electricity, and mechanical industries. Al2O3 dispersion-strengthened copper alloy uses copper as the main load-bearing component, and introduces Al2O3 as dispersed particles to hinder dislocation movement and inhibit recrystallization, thereby greatly improving the strength of the matrix. According to the different ways of introducing Al2O3 particles, the preparation process of Al2O3 dispersion-strengthened copper alloy materials can be divided into two categories: external particle method and in-situ reaction synthesis method. The external particle method includes powder metallurgy, mechanical alloying, composite electrodeposition, etc.; the in-situ reaction synthesis method includes internal oxidation, coprecipitation, sol-gel, etc. Among them, the internal oxidation method is currently the best method for large-scale production of Al2O3 dispersion-strengthened copper alloy materials. The process flow is: smelting to prepare Cu-Al alloy → water or N2 atomization to prepare Cu-Al alloy powder → Cu-Al and Cu2O powder are mixed in proportion → internal oxidation powder → excess oxygen is reduced in hydrogen → pressing → sintering and forming. The oxide particles obtained by this method are evenly distributed, and the reinforcing phase and the matrix interface are well bonded; the disadvantages are long production cycle, high cost, large Al2O3 particles, and it is difficult to adapt to industrial mass production. Mechanical alloying method: a high-energy ball mill is used to mix with fine Al2O3, and the powder is repeatedly deformed, fractured, welded, diffused between atoms or undergoes solid-state reaction through collision and extrusion of the grinding ball to form alloy powder, and then compacted, formed, sintered and extruded. This method has simple process, low cost, high output, and small Al2O3 particles; the disadvantage is that impurities are easily generated during the grinding process, pollution is difficult to obtain a clean crystal surface. Summary of the invention

[0003] The present invention provides a method for preparing an Al2O3 dispersion strengthened copper alloy material, which overcomes the above-mentioned deficiencies of the prior art and can effectively solve the problems of the prior art such as long production cycle, high cost, large Al2O3 particles, difficulty in adapting to industrial mass production and easy pollution.

[0004] The technical scheme of the present invention is achieved by the following measures: a preparation method of an Al2O3 dispersion strengthened copper alloy material, which is carried out according to the following steps: the first step is to mix copper powder, aluminum powder and CuO powder in proportion, add stearic acid and mix evenly to obtain a mixed powder, the amount of aluminum powder added is 0.2% to 2% of the mass of the mixed powder, the amount of CuO powder added is 5% to 10% of the mass of the mixed powder, and the amount of stearic acid added is 0.5% of the mass of the mixed powder, and then the mixed powder is added to a ball mill for a first ball milling, and a primary alloy powder is obtained after ball milling; the second step is to place the primary alloy powder in a vacuum sintering furnace for sintering treatment; the third step is to add 0.5% of the mass of the mixed powder after crushing and mix evenly, and perform secondary ball milling in a ball mill to obtain a secondary alloy powder after ball milling; the fourth step is to place the secondary alloy powder in a reduction furnace in a hydrogen atmosphere to reduce excess oxygen; the fifth step is to press and form after reduction treatment and place it in a vacuum sintering furnace again for sintering treatment, and the Al2O3 dispersion strengthened copper alloy material is obtained after treatment.

[0005] The following are further optimizations and / or improvements to the above technical solutions:

[0006] In the first step above, the purity of the copper powder is 99.95%, the purity of the aluminum powder is 99.9%, and the particle size of the CuO powder is less than 10 um.

[0007] In the first step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 55 minutes to 65 minutes, and the ball-to-material ratio of the ball mill is 5:1.

[0008] In the second step, the temperature of the vacuum sintering furnace is 850° C. to 950° C., and the sintering time is 1.5 hours to 2.5 hours.

[0009] In the third step, the rotation speed of the ball mill is 300 to 350 rpm, the ball milling time is 20 to 30 minutes, and the ball-to-material ratio of the ball mill is 5:1.

[0010] In the fifth step, the pressure of the pressing process is 750 MPa to 850 MPa; the temperature of the vacuum sintering furnace is 950° C. to 1050° C., and the sintering time is 1.5 hours to 2.5 hours.

[0011] The present invention combines mechanical alloying with internal oxidation for the first time, and obtains Al2O3 dispersion strengthened copper alloy material through mixed grinding, internal oxidation of mixed powder, secondary grinding, H2 removal of excess oxygen and pressing and sintering processes; compared with the existing process, the present invention greatly shortens the production cycle, has low production cost, less impurities, smaller Al2O3 particles, and is more adaptable to industrial mass production. Implementation

[0012] The present invention is not limited by the following embodiments, and specific implementation methods can be determined based on the technical solution of the present invention and actual conditions.

[0013] The present invention will be further described below in conjunction with embodiments:

[0014] Embodiment 1, the preparation method of the Al2O3 dispersion strengthened copper alloy material is carried out according to the following steps: the first step is to mix copper powder, aluminum powder and CuO powder in proportion, add stearic acid and mix evenly to obtain a mixed powder, the amount of aluminum powder added is 0.2% to 2% of the mass of the mixed powder, the amount of CuO powder added is 5% to 10% of the mass of the mixed powder, and the amount of stearic acid added is 0.5% of the mass of the mixed powder, and then the mixed powder is added to a ball mill for a first ball milling, and a primary alloy powder is obtained after ball milling; the second step is to place the primary alloy powder in a vacuum sintering furnace for sintering treatment; the third step is to add 0.5% of the mass of the mixed powder and mix evenly after sintering treatment, and perform secondary ball milling in a ball mill to obtain a secondary alloy powder; the fourth step is to place the secondary alloy powder in a reduction furnace in a hydrogen atmosphere to reduce excess oxygen; the fifth step is to press and form after reduction treatment and place it in a vacuum sintering furnace for sintering treatment again, and obtain Al2O3 dispersion strengthened copper alloy material after treatment. The primary alloy powder is Cu-Al-CuO alloy powder, and the particle size is relatively small.

[0015] Embodiment 2, as an optimization of the above embodiment, in the first step, the purity of the copper powder is 99.95%, the purity of the aluminum powder is 99.9%, and the particle size of the CuO powder is less than 10 um. The purity can be expressed as a mass percentage.

[0016] Example 3, as an optimization of the above example, in the first step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 55 minutes to 65 minutes, and the ball-to-material ratio of the ball mill is 5:1.

[0017] Embodiment 4, as an optimization of the above embodiment, in the second step, the temperature of the vacuum sintering furnace is 850° C. to 950° C., and the sintering time is 1.5 hours to 2.5 hours.

[0018] Example 5, as an optimization of the above example, in the third step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 20 minutes to 30 minutes, and the ball-to-material ratio of the ball mill is 5:1.

[0019] Example 6, as an optimization of the above example, in the fifth step, the pressure of the pressing process is 750Mpa to 850Mpa; the temperature of the vacuum sintering furnace is 950°C to 1050°C, and the sintering time is 1.5 hours to 2.5 hours.

[0020] Embodiment 7, the preparation method of the Al2O3 dispersion strengthened copper alloy material is carried out according to the following steps: the first step is to mix copper powder with a purity of 99.95%, aluminum powder with a purity of 99.9%, and CuO powder with a particle size of 8um in proportion, add stearic acid and mix evenly to obtain a mixed powder, the amount of aluminum powder added is 1.8% of the mass of the mixed powder, the amount of CuO powder added is 7% of the mass of the mixed powder, and the amount of stearic acid added is 0.5% of the mass of the mixed powder, and then add the mixed powder into a ball mill for a first ball milling, the speed of the ball mill is 350 rpm, the ball milling time is 50 minutes, and the ball-to-material ratio of the ball mill is 5:1, and a primary alloy powder is obtained after ball milling; the second step is to place the primary alloy powder in a vacuum sintering furnace The invention relates to a step of sintering, wherein the temperature of the vacuum sintering furnace is 950°C and the sintering time is 2 hours; the third step is to add 0.5% stearic acid by mass of the mixed powder after crushing and mix evenly, and to carry out secondary ball milling in a ball mill, wherein the speed of the ball mill is 300 rpm, the ball milling time is 30 minutes, and the ball-to-material ratio of the ball mill is 5:1, and secondary alloy powder is obtained after ball milling; the fourth step is to place the secondary alloy powder in a reduction furnace in a hydrogen atmosphere to reduce excess oxygen; the fifth step is to press and shape the powder after reduction treatment and place the powder in a vacuum sintering furnace for sintering treatment again, wherein the pressure during the pressing process is 750 MPa, the temperature of the vacuum sintering furnace is 1000°C, and the sintering time is 1.5 hours, and Al2O3 dispersion-strengthened copper alloy material is obtained after treatment. The Al2O3 dispersion-strengthened copper alloy material obtained in Example 7 has a production cycle shortened by 1 / 4 and a production cost reduced by 20% compared with the internal oxidation method. The Al2O3 particles are smaller and more suitable for industrial mass production. Compared with the mechanical alloying method, it is less likely to produce impurities during the grinding process and a clean crystal surface can be obtained.

[0021] Embodiment 8, the preparation method of the Al2O3 dispersion strengthened copper alloy material is carried out according to the following steps: the first step, copper powder with a purity of 99.95%, aluminum powder with a purity of 99.9%, and CuO powder with a particle size of 5um are mixed together in proportion, stearic acid is added and mixed evenly to obtain a mixed powder, the amount of aluminum powder added is 0.8% of the mass of the mixed powder, the amount of CuO powder added is 6% of the mass of the mixed powder, and the amount of stearic acid added is 0.5% of the mass of the mixed powder, and then the mixed powder is added to a ball mill for a ball milling, the speed of the ball mill is 350 rpm, the ball milling time is 60 minutes, the ball mill material ratio is 5:1, and a primary alloy powder is obtained after ball milling; the second step, the primary alloy powder is placed in a vacuum sintering furnace for The powder is sintered at a temperature of 950°C and a sintering time of 2.5 hours in a vacuum sintering furnace. The third step is to add 0.5% stearic acid by weight of the mixed powder after crushing and mix evenly, and then perform secondary ball milling in a ball mill at a speed of 300 rpm and a ball milling time of 25 minutes. The ball-to-material ratio of the ball mill is 5:1, and secondary alloy powder is obtained after ball milling. The fourth step is to place the secondary alloy powder in a reduction furnace in a hydrogen atmosphere to reduce excess oxygen. The fifth step is to press the powder after reduction and place it in a vacuum sintering furnace for sintering again. The pressure during the pressing process is 850 MPa, the temperature of the vacuum sintering furnace is 1050°C, and the sintering time is 2.5 hours. Al2O3 dispersion-strengthened copper alloy material is obtained after treatment. The Al2O3 dispersion-strengthened copper alloy material obtained in Example 8 has a production cycle shortened by 1 / 3 and a production cost reduced by 28% compared with the internal oxidation method. The Al2O3 particles are smaller and more suitable for industrial mass production. Compared with the mechanical alloying method, it is less likely to produce impurities during the grinding process and a clean crystal surface can be obtained.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] The preparation method of the Al2O3 dispersion-strengthened copper alloy material of the present invention is as follows: Cu-Al-CuO mixed grinding → mixed powder internal oxidation → secondary grinding - H2 gas to remove excess oxygen → pressing and sintering;

[0024] 1. Compared with the existing internal oxidation method, the present invention has a simple process, a short production cycle and low cost;

[0025] 2. The mechanical alloying method is used to prepare Cu-Al-CuO alloy powder, and the powder particles obtained are smaller;

[0026] 3. The particle size of CuO used in the present invention is required to be less than 10um. The finer the CuO particles are, the more conducive it is to generate Cu2O (CuO+Cu--Cu2O) during internal oxidation to provide a greater oxygen partial pressure;

[0027] 4. The Cu powder in the Cu-Al-CuO alloy powder of the present invention will react with CuO to generate Cu2O as an oxygen supply medium under high temperature conditions;

[0028] 5. In the present invention, the Al2O3 particles obtained by refining the powder by secondary grinding are smaller. The strength of Al2O3 dispersion-strengthened copper, especially the high-temperature strength, is closely related to the spacing and size of the dispersed Al2O3 particles.

[0029] In summary, the present invention combines the mechanical alloying method with the internal oxidation method for the first time, and obtains Al2O3 dispersion-strengthened copper alloy material through mixed grinding, internal oxidation of mixed powder, secondary grinding, H2 removal of excess oxygen and pressing and sintering processes; compared with the existing process, the present invention greatly shortens the production cycle, has low production cost, less impurities, smaller Al2O3 particles, and is more adaptable to industrial mass production.

[0030] The above technical features constitute the embodiments of the present invention, which have strong adaptability and implementation effect. Non-essential technical features can be added or reduced according to actual needs to meet the requirements of different situations.

Claims

1. A method for preparing an Al2O3 dispersion-strengthened copper alloy material, characterized in that The process is as follows: first, copper powder, aluminum powder and CuO powder are mixed together in proportion, stearic acid is added and mixed evenly to obtain a mixed powder, wherein the amount of aluminum powder added is 0.2% to 2% of the mass of the mixed powder, the amount of CuO powder added is 5% to 10% of the mass of the mixed powder, and the amount of stearic acid added is 0.5% of the mass of the mixed powder, and then the mixed powder is added to a ball mill for a first ball milling to obtain a primary alloy powder; second, the primary alloy powder is placed in a vacuum sintering furnace for sintering treatment; third, after the sintering treatment, the primary alloy powder is crushed, 0.5% of the mass of the mixed powder is added with stearic acid and mixed evenly, and a second ball milling is performed in a ball mill to obtain a secondary alloy powder; fourth, the secondary alloy powder is placed in a reduction furnace in a hydrogen atmosphere to reduce excess oxygen; fifth, after the reduction treatment, the powder is pressed into shape and placed in a vacuum sintering furnace for sintering treatment again to obtain an Al2O3 dispersion strengthened copper alloy material.

2. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 1, characterized in that In the first step, the purity of copper powder is 99.95%, the purity of aluminum powder is 99.9%, and the particle size of CuO powder is less than 10um.

3. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 1 or 2, characterized in that In the first step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 55 minutes to 65 minutes, and the ball-to-material ratio of the ball mill is 5:

1.

4. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 1 or 2, characterized in that In the second step, the temperature of the vacuum sintering furnace is 850° C. to 950° C., and the sintering time is 1.5 hours to 2.5 hours.

5. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 3, characterized in that In the second step, the temperature of the vacuum sintering furnace is 850° C. to 950° C., and the sintering time is 1.5 hours to 2.5 hours.

6. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 1 or 2, characterized in that In the third step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 20 minutes to 30 minutes, and the ball-to-material ratio of the ball mill is 5:

1.

7. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 5, characterized in that In the third step, the rotation speed of the ball mill is 300 rpm to 350 rpm, the ball milling time is 20 minutes to 30 minutes, and the ball-to-material ratio of the ball mill is 5:

1.

8. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 1 or 2, characterized in that In the fifth step, the pressure of the pressing process is 750Mpa to 850Mpa; the temperature of the vacuum sintering furnace is 950°C to 1050°C, and the sintering time is 1.5 hours to 2.5 hours.

9. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 3, characterized in that In the fifth step, the pressure of the pressing process is 750Mpa to 850Mpa; the temperature of the vacuum sintering furnace is 950°C to 1050°C, and the sintering time is 1.5 hours to 2.5 hours.

10. The method for preparing the Al2O3 dispersion strengthened copper alloy material according to claim 7, characterized in that In the fifth step, the pressure of the pressing process is 750Mpa to 850Mpa; the temperature of the vacuum sintering furnace is 950°C to 1050°C, and the sintering time is 1.5 hours to 2.5 hours.