A composite material based on zirconium-based metal-organic framework and Bi4O5I2 and its application

By using the composite material of zirconium-based metal organic frame and Bi4O5I2 for photocatalytic reactors, the unutilized problem of PCN-222/PCN-223 and Bi4O5I2 composite materials in the field of CO2 reduction in the prior art is solved, and efficient CO2 is achieved Reduction effect and excellent photocatalytic properties.

CN116651504BActive Publication Date: 2024-11-15ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310041020.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-11-15
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

The existing photocatalytic materials have not yet been used in the CO2 reduction field, which has led to the inadequate photocatalytic CO2 reduction performance being insufficiently utilized.

Method used

The composite material of zirconium-based metal organic frame (PCN-222 or PCN-223) and Bi4O5I2 is used to disperse and sonicate it in DMF, combined with specific preparation methods to form a composite material with good conductivity and photocatalytic CO2 reduction properties. Used for CO2 reduction in photocatalytic reactors.

Benefits of technology

It realizes high conversion rate catalyzing CO2 under mild conditions to generate CO products, and has excellent light absorption and conductivity, which significantly improves the photocatalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116651504B_ABST
    Figure CN116651504B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalytic materials, and discloses a composite material based on a zirconium-based metal organic framework and Bi4O5I2 and an application thereof. The composite material is obtained by reacting PCN‑222 / PCN‑223 and Bi4O5I2 as raw materials under DMF conditions. Compared with the prior art, the composite material of PCN‑222 / PCN‑223 and Bi4O5I2 prepared by the present invention has good light absorption performance and electrical conductivity, so that CO2 can be catalytically converted at a high conversion rate under mild conditions, and CO can be produced with high selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to the technical field of catalytic materials, in particular to a catalyst based on a zirconium-based metal organic framework and Bi 4 O 5 I 2 Composite materials and their applications in the field of photocatalytic carbon dioxide reduction. Background technology:

[0002] Under the dual pressure of environmental pollution and energy shortage, photocatalytic CO 2 Reduction technology has attracted much attention. The development of low-cost photocatalytic materials is crucial to achieve efficient solar-to-fuel conversion.

[0003] Metal-organic frameworks (MOFs) are organic-inorganic hybrid materials with intramolecular pores formed by self-assembly of organic ligands and metal ions or clusters through coordination bonds. As a new type of solid porous material, MOFs have the advantages of large specific surface area, high porosity, adjustable functions, adjustable host-guest interaction, and high stability, making them potential application values ​​in catalysis, sensing, gas separation, and adsorption and separation of small organic molecules.

[0004] Porphyrin has become one of the important organic ligands of MOFs due to its good photosensitivity and catalytic performance, as well as good thermal stability and chemical stability. Porphyrin-based MOFs can not only give full play to the excellent properties of MOFs structure, but also effectively enhance light absorption and photostability. Therefore, porphyrin-based MOFs have important application backgrounds in the fields of gas separation, storage, catalysis, luminescence and fluorescence detection.

[0005] In order to obtain a photocatalyst with better photocatalytic oxygen reduction performance, porphyrin and MOFs are combined to construct a non-precious metal photocatalyst with mutually compensatory and mutually promoting photocatalytic oxygen reduction activity. PCN-222 and PCN-223 are two three-dimensional porphyrin MOFs materials with one-dimensional pore structures that have been studied more in recent years. PCN-222 and PCN-223 molecules have low conductivity themselves, while Bi 4 O 5 I 2 As a new type of layered bismuth-based semiconductor material, it has attracted extensive attention in the field of photocatalysis in recent years. a O b X c The crystal is a double layer of halogen X ions and [Bi 2 O 2] layers are arranged alternately. In the [X-Bi-O-Bi-X] layer structure, bismuth atoms are surrounded by oxygen atoms and halogen atoms. Strong intralayer covalent bond forces and weak interlayer van der Waals interactions make Bi a O b X c Semiconductor materials have high anisotropy in structure, electronics, optics and mechanical properties. PCN-222 / PCN-223 and Bi with high conductivity 4 O 5 I 2 The combination can increase the material's electrical conductivity, thereby improving its photocatalytic properties.

[0006] However, PCN-222 / PCN-223 and Bi 4 O 5 I 2 Composite materials for photocatalytic CO 2 Its application in reduction has not been reported in the literature. Summary of the invention:

[0007] In view of the above technical problems existing in the prior art, in order to make full use of PCN-222 / PCN-223 and Bi 4 O 5 I 2 The invention provides a material based on a zirconium-based metal organic framework and Bi 4 O 5 I 2 Composite materials and applications thereof, the present invention provides a novel PCN-222 / PCN-223 and Bi 4 O 5 I 2 The composite material has good electrical conductivity and photocatalytic CO 2 Restore performance.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] The method is based on a zirconium-based metal organic framework and Bi 4 O 5 I 2 The composite material, wherein the zirconium-based metal organic framework is at least one of PCN-222 and PCN-223, and the zirconium-based metal organic framework and Bi 4 O 5 I 2 The product is dispersed in DMF at a mass ratio of 1:0.1-0.5, ultrasonicated at 100W for 1-3 hours, washed with acetone, and dried at 60-80°C for 10-20 hours to obtain the zirconium-based metal organic framework and Bi 4 O5 I 2 of composite materials.

[0010] The method is based on a zirconium-based metal organic framework and Bi 4 O 5 I 2 The composite material, the preparation method of PCN-222 or PCN-223 comprises the following steps:

[0011] 1) dissolving 5,10,15,20-(4-carboxyphenyl)porphyrin in DMF to form a solution;

[0012] 2) Add formic acid or propionic acid and ZrCl to the solution 4 , ultrasound for 10 to 20 minutes;

[0013] 3) transferring the solution of step 2) into an oven and reacting at 110-130° C. for 20-30 hours. After the reaction is completed, centrifuging to obtain a solid product;

[0014] 4) The product is washed with DMF and acetone in sequence, and then dried at 60-80° C. for 10-20 h to obtain the product PCN-222 or PCN-223.

[0015] Further, the 5,10,15,20-(4-carboxyphenyl)porphyrin in step 1) and the formic acid or propionic acid in step 2) and ZrCl 4 The mass ratio is 1:100~720:0.6~0.8.

[0016] Furthermore, the Bi 4 O 5 I 2 The preparation method comprises the following steps:

[0017] S1: dissolve KI in glycerol to obtain solution A;

[0018] S2: Change Bi(NO 3 ) 3 ·5H 2 O is dissolved in glycerol to obtain solution B;

[0019] S3: under continuous stirring, solution A is added dropwise to solution B, and after mixing evenly, the solution is placed in a polytetrafluoroethylene reactor, and then transferred to an oven for reaction at 150-170°C for 12-20h;

[0020] S4: After the reaction in step S3 is completed, the product is washed with ethanol and water in sequence, and then dried at 60-80°C for 10-20h to obtain the product Bi 4 O 5 I 2 .

[0021] The invention relates to a zirconium-based metal organic framework and Bi 4 O 5 I 2 Composite materials for photocatalytic conversion of CO 2 The invention relates to an application of the invention in generating CO by reaction, characterized in that the zirconium-based metal organic framework and Bi are added into a photocatalytic reactor. 4 O 5 I 2 The composite material and pure water, wherein the concentration of the composite material in the pure water is 0.2 to 1.0 g / L. The atmosphere in the reactor is replaced with CO 2 After the gas, CO 2 When the pressure in the reactor is 70-90 kPa and the reaction temperature is controlled at 5°C by condensing water, the reactor is irradiated and reacted under a 300W xenon lamp with stirring at 400-1000 rpm to generate CO products.

[0022] By adopting the above technical solution, the PCN-222 / PCN-223 and Bi 4 O 5 I 2 The composite material has good light absorption and electrical conductivity, and is suitable for photocatalytic CO 2 It works well as a photocatalyst in reduction.

[0023] In summary, the beneficial effects of the present invention are mainly reflected in: the present invention uses PCN-222 / PCN-223 and Bi 4 O 5 I 2 The composite material was used as a photocatalyst to photocatalyze CO 2 PCN-222 / PCN-223 and Bi 4 O 5 I 2 The composite material has excellent light absorption, free electron excitation and photocatalytic properties, and has good conductivity, and can catalyze the conversion of CO with high conversion rate under mild conditions. 2 , and produces CO with high selectivity. Description of the drawings:

[0024] Figure 1 PCN-222 and Bi obtained in Example 2 of the present invention 4 O 5 I 2 X-ray diffraction spectrum of the composite material;

[0025] Figure 2 PCN-222 and Bi obtained in Example 2 of the present invention 4 O5 I 2 Fourier transform infrared spectrum of the composite material;

[0026] Figure 3 PCN-222 and Bi obtained in Example 2 of the present invention 4 O 5 I 2 Transmission electron microscopy of composite materials;

[0027] Figure 4 PCN-222 and Bi obtained in Example 2 of the present invention 4 O 5 I 2 Transmission electron microscope element distribution map of the composite material;

[0028] Figure 5 PCN-222 and Bi obtained in Example 2 of the present invention 4 O 5 I 2 , PCN-222 and Bi 4 O 5 I 2 Photocatalytic reduction of CO by the composite material 2 Performance graph. Specific implementation method:

[0029] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereto:

[0030] Embodiment 1:

[0031] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4 (42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0032] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and then reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0033] PCN-222 (60 mg) and Bi 4 O 5 I 2 (6 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is that the CO production in 4 hours is 5.6 μmolCO / g catalyst, referred to as CO production of 5.6 μmol / g.

[0034] Embodiment 2:

[0035] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4 (42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0036] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0037] PCN-222 (60 mg) and Bi 4 O 5 I 2 (12 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The composite material; its XRD is as follows Figure 1 As shown, we can clearly see the peak of PCN-222, while Bi 4 O 5 I 2 The peak is not obvious, which is similar to the case in other composite materials literature; its infrared spectrum is as follows Figure 2 As shown, it can be found that PCN-222 and Bi 4 O 5 I 2 The composite material has both Bi 4 O 5 I 2 The key peak of PCN-222 also appeared at 1411cm -1 A broad peak appears at the -COO (symmetrical) bond because some -COO and Bi 4 O 5 I 2 Combined with the transmission electron microscope and element distribution diagram Figure 3 , Figure 4 As shown, transmission electron microscopy revealed that PCN-222 and Bi 4 O 5 I 2 The two materials are closely combined, and the element distribution diagram can clearly distinguish the two materials; Figure 5 As shown, the photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2The photocatalytic performance of the composite material was greatly improved, and the CO production in 4 hours was 28.6 μmol / g; therefore, the above tests can determine that PCN-222 and Bi 4 O 5 I 2 Successful preparation of composite materials;

[0038] Embodiment 3:

[0039] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4 (42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0040] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.97 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0041] PCN-222 (60 mg) and Bi 4 O 5 I 2 (18 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 20.5 μmol / g in 4 hours.

[0042] Embodiment 4:

[0043] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4 (42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0044] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0045] PCN-222 (60 mg) and Bi 4 O 5 I 2 (24 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 15.3 μmol / g in 4 hours.

[0046] Embodiment 5:

[0047] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4 (42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0048] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0049] PCN-222 (60 mg) and Bi 4 O 5 I 2 (30 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 13.2 μmol / g in 4 hours.

[0050] Embodiment 6:

[0051] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Formic acid (10 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-222.

[0052] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0053] PCN-222 (60 mg) and Bi 4 O 5 I 2 (12 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 2 hours. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 27.8 μmol / g in 4 hours.

[0054] Embodiment 7:

[0055] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0056] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0057] PCN-223 (60 mg) and Bi 4 O 5 I 2 (6 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-223 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 3.5 μmol / g in 4 hours.

[0058] Embodiment 8:

[0059] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0060] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0061] PCN-223 (60 mg) and Bi 4 O 5 I 2 (12 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-223 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 14.5 μmol / g in 4 hours.

[0062] Embodiment 9:

[0063] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0064] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.97 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0065] PCN-223 (60 mg) and Bi 4 O 5 I 2 (18 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-222 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 12.8 μmol / g in 4 hours.

[0066] Embodiment 10:

[0067] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0068] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0069] PCN-223 (60 mg) and Bi 4 O 5 I 2 (24 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-223 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 8.5 μmol / g in 4 hours.

[0070] Embodiment 11:

[0071] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0072] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0073] PCN-223 (60 mg) and Bi 4 O 5 I 2 (30 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 1 hour. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-223 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is 6.2 μmol / g of CO production in 4 hours.

[0074] Embodiment 12:

[0075] 5,10,15,20-(4-carboxyphenyl)porphyrin (60 mg) was dissolved in DMF (20 ml) to form a solution, and the solution was sonicated for 10 min. Propionic acid (6 ml) and ZrCl were added to the solution. 4(42 mg), and continue ultrasonication for 10 minutes. The solution was placed in an oven and reacted at 120°C for 24 hours. After the reaction was completed, the solid product was obtained by centrifugation. The product was first washed 3 times with DMF (20 ml), then washed 3 times with acetone (20 ml), and finally the obtained solid product was placed in an oven and dried at 70°C for 12 hours to obtain the product PCN-223.

[0076] KI (0.332 g) was dissolved in glycerol (20 ml) to obtain solution A; Bi(NO 3 ) 3 ·5H 2 O (0.970 g) was dissolved in glycerol (20 ml) to obtain solution B. Solution A was added dropwise to solution B under continuous stirring. After mixing evenly, the solution was placed in a polytetrafluoroethylene reactor and reacted in an oven at 160 °C for 16 h. The product was washed with ethanol for 3 to 5 times and then with H 2 O for 3 to 5 times, and finally put the obtained solid into a vacuum drying oven and dry it at 70°C for 12 hours. 4 O 5 I 2 .

[0077] PCN-223 (60 mg) and Bi 4 O 5 I 2 (12 mg) was dispersed in DMF, and the solution was ultrasonicated at 100 W for 3 hours. The product was washed with acetone for 3 to 5 times, and finally the obtained solid was placed in an oven and dried at 70 ° C for 12 hours. PCN-223 and Bi 4 O 5 I 2 The photocatalytic carbon dioxide reduction performance test shows that PCN-222 and Bi 4 O 5 I 2 The photocatalytic performance of the composite material is a CO production of 14.3 μmol / g in 4 hours.

[0078] Embodiment 13:

[0079] A PCN-222 / PCN-223 and Bi 4 O 5 I 2 The application of the composite material in photocatalytic carbon dioxide reduction, the specific steps are:

[0080] The photocatalytic reaction was carried out in a specially prepared reactor containing 30 mg of one of the catalysts in Examples 1 to 12 and 50 mL of pure water. 2The gas was inflated and deflated three times, and CO was introduced into the reactor after three times. 2 The pressure in the reactor was 80 kPa and the reaction temperature was 5° C. The reactor was then irradiated with a 300 W xenon lamp at 600 rpm. The gas in the reactor was sampled into a gas chromatograph every 1 h to determine the amount of the product.

[0081] PCN-222 and Bi obtained in Example 2 of the present invention 4 O 5 I 2 , PCN-222 and Bi 4 O 5 I 2 Photocatalytic reduction of CO by the composite material 2 Performance diagram Figure 5 shown.

[0082] Obviously, the above embodiments are only examples for clearly explaining the content of the present invention, rather than limiting the implementation methods. For those skilled in the art, based on the above description, PCN-222 / PCN-223 with other metals introduced into the porphyrin center can also be made. It is not necessary and impossible to give examples of all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of the present invention.

Claims

1. A novel Zr-based metal-organic framework and Bi 4 O 5 I 2 Composite materials for photocatalytic conversion of CO 2 Application in the reaction to generate CO, Features: The zirconium-based metal organic framework is PCN-222, and the zirconium-based metal organic framework and Bi 4 O 5 I 2 The mixture is dispersed in DMF at a mass ratio of 1:0.1-0.5, ultrasonicated for 1-5 hours, washed with acetone, and dried at 60-80 °C for 10-20 hours to obtain the zirconium-based metal organic framework and Bi 4 O 5 I 2 of composite materials.

2. The use according to claim 1, Features: The preparation method of PCN-222 comprises the following steps: 1) dissolving 5,10,15,20-(4-carboxyphenyl)porphyrin in DMF to form a solution; 2) Add formic acid and ZrCl to the solution 4 , ultrasound for 10 to 20 minutes; 3) The solution of step 2) is transferred into an oven and reacted at 110-130°C for 20-30 hours. After the reaction is completed, the solid product is obtained by centrifugation; 4) The product is washed with DMF and acetone in sequence, and then dried at 60-80 °C for 10-20 h to obtain the product PCN-222.

3. The use according to claim 2, Features: 5,10,15,20-(4-carboxyphenyl)porphyrin in step 1) and formic acid and ZrCl in step 2) 4 The mass ratio is 1:100~720:0.6~0.

8.

4. The use according to claim 1, Features: The Bi 4 O 5 I 2 The preparation method comprises the following steps: S1: dissolve KI in glycerol to obtain solution A; S2: Change Bi(NO 3 ) 3 ·5H 2 O is dissolved in glycerol to obtain solution B; S3: Under continuous stirring, solution A is added dropwise to solution B. After mixing evenly, the solution is placed in a polytetrafluoroethylene reactor and then transferred to an oven for reaction at 150-170 °C for 12-20 h. S4: After the reaction in step S3 is completed, the product is washed with ethanol and water in sequence, and then dried at 60-80 °C for 10-20 h to obtain the product Bi 4 O 5 I 2 .

5. The use according to claim 1, Features: The zirconium-based metal organic framework and Bi are added to the photocatalytic reactor 4 O 5 I 2 The atmosphere in the reactor was replaced with CO 2 After the gas, CO 2 The pressure in the reactor was 70-90 kPa, and the reaction temperature was controlled at 5 °C by condensing water. The reactor was then irradiated with a 300 W xenon lamp and stirred at 400-1000 rpm to generate CO products.

6. The use according to claim 5, Features: The concentration of the composite material in pure water is 0.2-1.0 g / L.