A nylon material and preparation method thereof
By using suitable free radical quenchers and acid respirators in halogen-free flame retardant nylon materials, the precipitation and degradation of flame retardants are suppressed, and the rubber aging problem caused by flame retardants is solved, achieving good in humid and hot environments Sealing performance and long-term stability.
Patent Information
- Application Number
- CN202310569184.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-19
AI Technical Summary
Halogen-free flame-retardant nylon materials are easily precipitated during long-term use, especially in humid and hot environments, resulting in accelerated aging and failure of the rubber seal ring, and cannot effectively inhibit the degradation reaction between the flame retardant and rubber.
Use suitable radical quenchers and acid respirators to inhibit the precipitation of flame retardant in halogen-free flame retardant nylon materials, bind hindered amine compounds to the rubber chain free radicals, slow down the degradation of rubber molecular chains, and through specific Component ratios and process conditions improve material properties.
It effectively inhibits the degradation reaction between flame retardant and rubber, maintains the good elasticity and sealing performance of the rubber sealing ring after long-term use and humidity and heat aging, and extends the service life of the material.
Smart Images

Figure BDA0004237788540000021 
Figure BDA0004237788540000041 
Figure BDA0004237788540000042
Abstract
Description
Technical Field
[0001] The invention belongs to the field of modified plastics, and in particular relates to a nylon material and a preparation method thereof. Background Art
[0002] Rubber sealing materials are currently the most widely used sealing materials due to their excellent elasticity, corrosion resistance, simple manufacturing process, and low cost. When compressed, rubber undergoes elastic deformation, contraction-elastic deformation that attempts to return to its original shape, and plastic deformation. These elastic and contraction-elastic deformations are the mechanisms by which rubber achieves its sealing function. However, under long-term stress or when the rubber itself ages or even becomes brittle, elastic deformation transforms into plastic deformation, causing seal failure. Rubber types used to manufacture sealing rings include silicone rubber, fluororubber, polyacrylate rubber, butyl rubber, ethylene propylene rubber, and styrene butadiene rubber.
[0003] Flame-retardant nylon materials achieve specific levels of flame retardancy through the introduction of flame retardants. Common flame-retardant nylon materials on the market can be divided into two categories based on the type of flame retardant: bromine-based flame retardant and halogen-free. Halogen-free flame retardant materials can be further divided into phosphorus-based flame retardant, nitrogen-based flame retardant, and intumescent flame retardant. Bromine-based flame-retardant nylon materials are subject to environmental regulations, but their low CTI values also limit their use in high-voltage electrical equipment and components. Halogen-free flame-retardant nylon materials, with CTI values up to 600V, meet environmental regulations and are widely used in high-voltage electrical applications. During long-term use, especially in hot and humid environments, the halogen-free flame retardant easily precipitates and accumulates on the surface of halogen-free flame-retardant nylon materials, accelerating aging and even causing brittleness and failure of rubber seals in contact with them.
[0004] Patent CN201811440424.4 introduces a chain scission agent into the hypophosphite flame-retardant nylon system to reduce the shearing of the flame retardant during the extrusion process, reduce the proportion of flame retardant decomposition and the production of small molecules, and thus reduce the precipitation of flame retardants during the use of flame-retardant nylon materials. Similarly, patent CN201811440417.4 introduces a substance that restricts the movement of nylon molecular chains, restricts the entry and exit of water into the resin matrix, and further uses a flame retardant precipitation inhibitor to produce water during the extrusion process to break the nylon molecular chain, thereby reducing the shearing of the flame retardant during the extrusion process. Patent CN201911306473.3 uses a surface-modified nitrogen-based flame retardant and compounds it with a flame retardant toughening agent containing flame retardant elements to improve the compatibility of the flame retardant component with nylon, solving the problem of flame retardant precipitation in flame-retardant nylon products. However, when the nylon material with improved flame retardant precipitation comes into contact with the rubber sealing ring for a long time, the flame retardant contained in the flame retardant nylon material will still cause the rubber to degrade and harden. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a nylon material and a preparation method thereof. By selecting a suitable free radical quencher and combining it with an acid absorber, the flame retardant precipitated from the halogen-free flame retardant nylon material is suppressed, thereby essentially curbing the degradation reaction between the flame retardant and the rubber.
[0006] The present invention provides a nylon material comprising the following components in parts by mass:
[0007]
[0008] The free radical quencher is a hindered amine compound, the molecular structure of which is a tetramethylpiperidinyl derivative and the molecular weight is 400-3100 g / mol.
[0009] The tetramethylpiperidinyl derivative can combine with chain free radicals generated by degradation of rubber under the influence of flame retardants, thereby inhibiting further degradation of rubber molecular chains.
[0010] The polyamide resin is at least one of PA66 and PA6 resins, with a relative viscosity of 2.0-3.2 (test temperature 25° C., solvent 96% sulfuric acid). Preferably, the mass ratio of the PA66 to PA6 resins is 3-7:1.
[0011] The halogen-free flame retardant is at least one of red phosphorus, aluminum hypophosphite, aluminum diethylphosphinate, ammonium polyphosphate, melamine, and melamine cyanurate.
[0012] The glass fibers have an average diameter of 7-13 microns and an average length of 1.5-5 mm.
[0013] The heat stabilizer is at least one of phenolic heat stabilizers, thiosulfate esters, and aromatic amines.
[0014] The lubricant is at least one of hyperbranched polyester, stearate, ethylene bisstearamide, and polyethylene wax.
[0015] The acid scavenger is at least one of zinc borate, hydrotalcite, anhydrous sodium carbonate, carbodiimide, polycarbodiimide, and alkaline earth metal carbonate, preferably zinc borate and hydrotalcite.
[0016] Preferably, the polyamide resin comprises 37.5-48.5 parts; the glass fiber comprises 20-30 parts; the free radical quencher comprises 0.5-1.5 parts; and the acid absorbent comprises 0.5-1.5 parts.
[0017] The present invention also provides a method for preparing a halogen-free flame-retardant nylon material, comprising the following steps:
[0018] The components are added into a mixer and mixed evenly to obtain a uniformly mixed material; the uniformly mixed material is extruded and granulated through a twin-screw extruder to obtain a halogen-free flame-retardant nylon material; wherein the twin-screw extruder is set at a temperature of 220-280° C. and a screw speed of 200-600 rpm.
[0019] The present invention also provides an application of halogen-free flame-retardant nylon material in components used in contact with rubber sealing rings, such as new energy vehicle charging guns, charging sockets, connectors, etc. made of halogen-free flame-retardant nylon material as raw materials.
[0020] Beneficial effects
[0021] The present invention selects a suitable free radical quencher and combines it with an acid absorber. The acid absorber can neutralize the small molecular phosphoric acid produced by the degradation of the flame retardant in the halogen-free flame-retardant nylon material, thereby slowing down the degradation of the rubber in contact with the acidic conditions. At the same time, since rubber cannot completely avoid the influence of the flame retardant, a small amount of chain free radicals will be generated under the influence of the flame retardant. The free radical quencher can combine with the chain free radicals to inhibit the further degradation of the rubber molecular chain. Therefore, the present invention can meet the requirements of the rubber sealing ring still having good elasticity and sealing performance after long-term use and wet heat aging. DETAILED DESCRIPTION
[0022] Below in conjunction with specific embodiment, further set forth the present invention.Should be understood that these embodiments are only used to illustrate the present invention and are not used in limiting the scope of the present invention.In addition, should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall equally within the scope limited by the appended claims of the application.
[0023] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0024] The raw materials used in the following examples and comparative examples are as follows:
[0025] PA66 resin: from Huafeng Group, typical grade EP-158, relative viscosity 2.7;
[0026] PA6 resin: from Haiyang Chemical Fiber, typical brand HY 2800, relative viscosity 2.8;
[0027] Glass fiber: from Chongqing Composite Materials, brand ECS301HP-3-H, diameter 10um, length 3mm;
[0028] Heat stabilizer: phenolic heat stabilizer and thiosulfate antioxidant are compounded in a mass ratio of 1:1;
[0029] Halogen-free flame retardant: It is compounded by aluminum diethylphosphinate and melamine cyanurate in a mass ratio of 3:1;
[0030] Aluminum diethylphosphinate, from Qingdao Oupure New Materials Co., Ltd., typical brand is ADP-33P;
[0031] Melamine cyanurate, from Sichuan Fine Chemicals, typical brand is MCA-01;
[0032] Free radical quencher 1: polymeric high molecular weight hindered amine compound, typical brand is UV 944, molecular weight is 2500g / mol;
[0033] Free radical quencher 2: low molecular weight hindered amine compound, typical brand UV 770, molecular weight 480g / mol; acid scavenger 1: anhydrous sodium carbonate, molecular weight 106g / mol, chemically pure;
[0034] Acid scavenger 2: zinc borate, molecular weight 314 g / mol, chemically pure;
[0035] Lubricant: Hyperbranched polyester, commercially available.
[0036] The composite materials of each embodiment and comparative example were prepared by the following process:
[0037] The components are added into a mixer and mixed evenly to obtain a uniformly mixed material; the uniformly mixed material is extruded and granulated through a twin-screw extruder to obtain a halogen-free flame-retardant nylon material; wherein the twin-screw extruder is set at a temperature of 220-280° C. and a screw speed of 200-600 rpm.
[0038] The examples and comparative examples were subjected to the following test methods or test standards:
[0039] By combining silicone rubber with different contact materials and placing them in a rubber compression set apparatus (ASTM D395-2003, compression set, standard rubber specimen is a cylinder with a height of 6.0±0.2mm and a diameter of 13.0±0.2mm), and further testing the rubber's thermal permanent deformation through accelerated aging, the resilience of the silicone rubber can be quantitatively characterized, reflecting its sealing effect in actual use.
[0040] Vertical burning test: According to UL94 standard, sample size is 125mm*13mm*1.6mm, 125mm*13mm*3.2mm.
[0041] Table 1 Examples and Comparative Examples
[0042]
[0043] Table 2 Performance of Examples and Comparative Examples
[0044]
[0045] The nylon materials obtained in Examples 1-12 had air heat aging deformation rates of 7.2%-15.3% at 168 hours, 11.3%-16.5% at 336 hours, 16.1%-20.1% at 504 hours, and 20.9%-22.9% at 1000 hours. The nylon materials obtained in Examples 1-12 had air heat aging deformation rates of 7.1%-14.8% at 168 hours, 11.8%-17.1% at 336 hours, 14.3%-20.5% at 504 hours, and 15.3%-24.1% at 1000 hours.
[0046] Comparison of Example 1 and Comparative Example 3 shows that when the silicone rubber is in contact with the halogen-free flame-retardant nylon material and is aged at 150°C / 1000 hours or 85°C / 85% humidity, the permanent deformation of the silicone rubber reaches the maximum value (40%) of the rubber compression permanent deformation device, and the silicone rubber hardens and loses its elasticity.
[0047] It can be seen from Example 1 and Comparative Examples 1 and 2 that the halogen-free flame-retardant nylon material to which a free radical quencher or an acid scavenger is added reduces the permanent compression set of the silicone rubber in contact with the halogen-free flame-retardant nylon material after aging; and from Examples 1-12, it can be seen that when the free radical quencher and the acid scavenger are used in combination, the permanent deformation of the silicone rubber in contact with the halogen-free flame-retardant nylon material after aging is further improved.
Claims
1. Application of nylon material in parts that come into contact with rubber sealing rings. Features: The nylon material comprises the following components by mass: 30-80 parts of polyamide resin; 10-30 parts of halogen-free flame retardant; Glass fiber 1-50 parts; Heat stabilizer 0.4-0.8 parts; Lubricant 0.2-0.6 parts; 0.1-3 parts of free radical quencher; Acid absorbent 0.1-3 parts; Among them, the free radical quencher is a hindered amine compound, the molecular structure is a tetramethylpiperidinyl derivative, and the molecular weight is 2500-3100 g / mol; the halogen-free flame retardant is two of diethyl aluminum phosphinate and melamine cyanurate; the acid absorber is at least one of zinc borate, hydrotalcite, anhydrous sodium carbonate, carbodiimide, and polycarbodiimide.
2. The use according to claim 1, Features: The polyamide resin is at least one of PA66 and PA6 resins, and has a relative viscosity of 2.0-3.
2.
3. The use according to claim 2, Features: The mass ratio of the PA66 to PA6 resin is 3-7:
1.
4. The use according to claim 1, Features: The glass fibers have an average diameter of 7-13 microns and an average length of 1.5-5 mm.
5. The use according to claim 1, Features: The heat stabilizer is at least one of phenolic heat stabilizers, thiosulfate, and aromatic amines; the lubricant is at least one of hyperbranched polyester, stearate, ethylene bis stearamide, and polyethylene wax.
6. The use according to claim 1, Features: The polyamide resin comprises 37.5-48.5 parts; the glass fiber comprises 20-30 parts; the free radical quencher comprises 0.5-1.5 parts; and the acid absorber comprises 0.5-1.5 parts.
7. The use according to claim 1, Features: The preparation method of the nylon material comprises the following steps: The components are added into a mixer for mixing; the mixed materials are extruded and granulated through a twin-screw extruder to obtain a nylon material; wherein the twin-screw extruder is set at a temperature of 220-280° C. and a screw speed of 200-600 rpm.