Dual-purpose environmentally friendly solvent-free two-component polyurethane waterproof coating and preparation method and application thereof

By reacting diphenylmethane diisocyanate with polyether polyol and water to form a crosslinked polymer, the problems of toxic solvents and crosslinking agents in existing polyurethane waterproof coatings were solved, and two-component polyurethane waterproofing with excellent performance and environmental protection were developed. Paint, suitable for a variety of construction scenarios.

CN116676036BActive Publication Date: 2024-11-12HUNAN SHENYU NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310531147.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

Toxic and harmful solvents and crosslinking agents are often used in existing polyurethane waterproof coatings, which lead to environmental pollution and human health hazards. At the same time, the performance is insufficient, the construction is difficult, and it is difficult to meet the application needs.

Method used

Use diphenylmethane diisocyanate (MDI) instead of toluene diisocyanate, combines the first and second polyether polyols, water and fillers, and reacts water with MDI to generate a crosslinking polymer, abandoning coal tar and toxic solvents , improves environmental protection and performance.

Benefits of technology

It has achieved the development of environmentally friendly solvent-free two-component polyurethane waterproof coatings, excellent performance and low cost, suitable for wet interfaces and flat construction, solving the problems of sag and uneven thickness, and the production process is safe and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a dual-purpose, environmentally friendly, solvent-free, two-component polyurethane waterproof coating, and a preparation method and application thereof, and relates to the field of coatings. The raw materials used in the polyurethane waterproof coating include the following components: component A: a first polyether polyol and diphenylmethane diisocyanate; component B: a second polyether polyol, a filler, water, and a catalyst. The above-mentioned polyurethane waterproof coating has excellent performance and relatively low cost, and can be used for wet interface construction, while solving the problem of easy sagging in facade construction, and the problem of thin upper part and thick lower part. In addition, the polyurethane waterproof coating of the present invention has excellent leveling properties and can also be used for plane construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane coatings, and in particular to a dual-purpose, environment-friendly, solvent-free, two-component polyurethane waterproof coating and a preparation method and application thereof. Background Art

[0002] At present, polyurethane waterproof coatings containing coal tar and volatile toxic and harmful solvents have been eliminated. Although relevant scientific research units and manufacturers have developed some products to replace coal tar polyurethane waterproof coatings, they still need to use volatile organic solvents such as toluene and xylene as diluents to adjust viscosity and improve construction performance; at the same time, polyurethane waterproof coatings generally use 3,3′-dichloro-4,4′-diaminodiphenylmethane (MOCA) as a crosslinker. This substance is a white to light yellow crystalline powder, toxic and carcinogenic, and also has the risk of combustion and explosion. When heated to above 200°C or burned, MOCA will generate toxic and corrosive fumes containing hydrogen chloride and nitrogen oxides; in addition, polyurethane waterproof coatings generally use toluene diisocyanate (TDI) as the main raw material, and TDI is a highly toxic and dangerous substance with a strong pungent smell, and has strict requirements for use and transportation. The above-mentioned raw materials that are indispensable in the production and application of polyurethane waterproof coatings are all toxic substances that seriously pollute the environment and endanger human health.

[0003] At present, some units have also developed polyurethane waterproof coatings that do not contain MOCA or TDI. However, due to the lack of these two components, the performance of the developed polyurethane waterproof coatings has been reduced, and they are prone to sagging during construction, and the upper part is thin and the lower part is thick, which cannot meet application requirements.

[0004] Therefore, it is urgent to develop a new type of environmentally friendly polyurethane waterproof coating. Summary of the invention

[0005] The first technical problem to be solved by the present invention is:

[0006] Provided is a polyurethane waterproof coating.

[0007] The second technical problem to be solved by the present invention is:

[0008] Provided is a method for preparing the polyurethane waterproof coating.

[0009] The third technical problem to be solved by the present invention is:

[0010] Application of the polyurethane waterproof coating.

[0011] In order to solve the first technical problem, the technical solution adopted by the present invention is:

[0012] A polyurethane waterproof coating, wherein the raw materials used to prepare the polyurethane waterproof coating include component A and component B;

[0013] The component A comprises a first polyether polyol and diphenylmethane diisocyanate;

[0014] The component B comprises a second polyether polyol, a filler, water and a catalyst.

[0015] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0016] 1. The polyurethane waterproof coating of the present invention, wherein component A is a polymer prepolymer produced by the reaction of diphenylmethane diisocyanate (MDI) and a first polyether polyol, and its terminal group contains a certain amount of isocyanate (-NCO); component B is a curing system, and water and diphenylmethane diisocyanate (MDI) will quickly cure under high temperature conditions. The polyurethane waterproof coating of the present invention abandons coal tar components and does not contain toxic and harmful solvents such as toluene and xylene, greatly improving the environmental friendliness of the product.

[0017] 2. The present invention adopts diphenylmethane diisocyanate (MDI) to replace toluene diisocyanate (TDI) in the existing polyurethane waterproof coating. Usually, the isocyanate in the polyurethane waterproof coating adopts toluene diisocyanate (TDI), which is a colorless or slightly yellow transparent liquid at room temperature, has a strong irritating smell, is an extremely toxic and dangerous substance, has strict requirements for transportation, and is difficult to meet the following standards: the vapor pressure is less than 0.02 mg / L in an 8h working environment. The diphenylmethane diisocyanate (MDI) used in the present invention is similar to the molecular structure of TDI in terms of molecular structure, both contain two identical functional groups-NCO, and the molecular weight of MDI is larger than that of TDI, is liquid at room temperature, and has a freezing point of 10-15°C. MDI is a non-dangerous substance, has low volatility, no irritating odor, and a vapor pressure (25°C) of 0.012 Pa. It is relatively less toxic to the human body, has no special requirements for transportation, has no irritating odor and pollution during production and construction, and is conducive to industrial safety protection.

[0018] 3. The present invention does not need to add an additional crosslinking agent, and does not need to add 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA). The present invention uses diphenylmethane diisocyanate to react with water to prepare a polymer with crosslinking ability. The reaction principle is as follows: first, diphenylmethane diisocyanate reacts with water to generate unstable carbamic acid, and then the carbamic acid decomposes into carbon dioxide and amine. Further, the generated amine continues to react with diphenylmethane diisocyanate to generate urea. The reaction process is as follows:

[0019] nONC-R-NCO+2nH2O→nHOOCNH-R-NHCOOH→nH2N-R-NH2+2nCO2;

[0020] nONC-R-NCO+nH2N-R-NH2→(NH-R-NHCONH-R-NHCO)n;

[0021] Since the reaction between R—NH2 and R—NCO is faster than that between water, the above reaction can be written as:

[0022] 2nONC-R-NCO+2nH20→(NH-R-NHCONH-R-NHCO) n +2nCO2.

[0023] Here, R represents a hydrocarbon group or an alkyl group.

[0024] It can be seen from the above reaction formula that one water molecule can react with two -NCO groups, that is, water can be regarded as a chain extender or curing agent, which can replace MOCA to extend the molecular chain and form a polymer with cross-linking ability.

[0025] 3. The polyurethane waterproof coating has excellent performance, relatively low cost, and can be used for wet interface construction, while solving the problem of easy sagging in facade construction, thin upper part and thick lower part. In addition, the polyurethane waterproof coating of the present invention has excellent leveling properties and can also be used for plane construction.

[0026] According to one embodiment of the present invention, the raw materials used in the polyurethane waterproof coating include the following components in parts by weight:

[0027] Component A: 70-100 parts of a first polyether polyol, 20-30 parts of diphenylmethane diisocyanate;

[0028] Component B: 45-60 parts of the second polyether polyol, 40-60 parts of filler, 6-10 parts of water and 2-5 parts of catalyst.

[0029] According to one embodiment of the present invention, the first polyether polyol and the first polyether polyol are independently selected from at least one of polyether polyol 330N, polyether polyol 2000D, polyether polyol 1000D and polyether polyol 400D.

[0030] Among them, polyether polyol 2000D is used to improve elongation, polyether polyol 1000D is used to improve strength, and polyether polyol 400D is used to improve elongation. The present invention selects polyethers with low hydroxyl value and small molecular weight, and the viscosity is low, the synthetic material is not thick, and the construction is convenient.

[0031] According to one embodiment of the present invention, the filler is an inorganic powder filler, and the inorganic powder filler includes ordinary silicate cement 300 mesh, carbon black 300 mesh, heavy calcium carbonate powder 2000 mesh, talcum powder 1250 mesh, and light calcium carbonate powder 800 mesh. The mesh number of the inorganic powder filler is less than 800, which is conducive to easy separation.

[0032] According to one embodiment of the present invention, the component A further comprises 10-30 parts by weight of a plasticizer; and the component B further comprises 9-20 parts by weight of a plasticizer.

[0033] According to one embodiment of the present invention, the plasticizer is selected from at least one of synthetic plant esters (environmentally friendly plasticizers), dioctyl phthalate DOP, dibutyl phthalate DBP, and No. 52 chlorinated paraffin. The present invention selects a low-viscosity synthetic plant ester plasticizer.

[0034] According to one embodiment of the present invention, the component B further comprises the following components in parts by weight:

[0035] 1-5 parts of surfactant and 1-2 parts of thixotropic agent.

[0036] According to one embodiment of the present invention, the filler includes at least one of silicate cement, heavy calcium carbonate powder, talcum powder and light calcium carbonate powder.

[0037] According to one embodiment of the present invention, the fineness of the filler is 300-1250 meshes.

[0038] In order to make the polyurethane waterproof coating of the present invention have good construction performance, the key is that the A and B components must have appropriate viscosity. According to the test, when the prepolymer of the A component is polymerized, low molecular weight polyether polyol should be used as much as possible. In the B component, the viscosity is adjusted by adding a variety of light and easily dispersible fillers, and selecting a softener and functional additives (defoaming agent, anti-settling agent) of appropriate viscosity according to the temperature. It is also possible to add a suitable amount of water during construction and stir evenly to make it moderate in viscosity and good in homogeneity.

[0039] In order to solve the second technical problem, the technical solution adopted by the present invention is:

[0040] A method for preparing the polyurethane waterproof coating comprises the following steps:

[0041] Mixing a first polyether polyol and diphenylmethane diisocyanate, and heating to obtain the component A;

[0042] Mixing a second polyether polyol, a filler, water and a catalyst to obtain the component B;

[0043] The component A and the component B are mixed in a weight ratio of 1-2:2-4 to obtain the polyurethane waterproof coating.

[0044] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0045] 1. The method for preparing the polyurethane waterproof coating of the present invention does not require high-temperature vacuum dehydration, has low energy consumption, short production time, and no waste gas release.

[0046] 2. The production process technology of both component A and component B of the present invention adopts normal temperature stirring, which reduces production energy consumption; the whole production process meets environmental protection requirements, basically no three wastes are generated, and material loss is very small. However, the existing polyurethane production process requires strict heating and dehydration of various raw materials, has many operation links, and is greatly affected by temperature and time.

[0047] According to one embodiment of the present invention, the heating temperature is 60-80°C.

[0048] According to one embodiment of the present invention, the following steps are also included: maintaining the temperature for 2 to 3 hours after heating, and then cooling to 50-60°C.

[0049] Another aspect of the present invention also relates to the application of the polyurethane waterproof coating in waterproofing of roofing projects, including the polyurethane waterproof coating as described in the first embodiment. Since the application adopts all the technical solutions of the polyurethane waterproof coating, it at least has all the beneficial effects brought by the technical solutions of the above embodiments.

[0050] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0052] Figure 1 This is a tensile strength test diagram of the polyurethane waterproof coating prepared in Examples 1-3;

[0053] Figure 2 This is a test chart of the elongation at break of the polyurethane waterproof coating prepared in Examples 1-3. DETAILED DESCRIPTION

[0054] Embodiments of the present invention are described in detail below, examples of the above embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0055] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0056] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0057] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0058] In the examples, polyether polyol 330N, polyether polyol 2000D, polyether polyol 1000D and polyether polyol 400D were purchased from Bluestar Dongda.

[0059] In the embodiment, the parameter specifications of the raw materials selected are shown in Table 1.

[0060] Table 1

[0061]

[0062] Example 1

[0063] A polyurethane waterproof coating comprises the following components:

[0064] Component A: 70 parts of a first polyether polyol, 25 parts of diphenylmethane diisocyanate and 10 parts of a plasticizer;

[0065] The first polyether polyol includes 32 parts of polyether polyol 330N, 26 parts of polyether polyol 2000D, 6 parts of polyether polyol 1000D, 6 parts of polyether polyol 400D, and 10 parts of dioctyl phthalate DOP.

[0066] Component B: 45 parts of the second polyether polyol, 35 parts of filler, 5 parts of pigment, 6 parts of water, 2 parts of catalyst, 9 parts of plasticizer, 1 part of Tween and 1 part of thixotropic agent;

[0067] The second polyether polyol includes 20 parts of polyether 330N and 25 parts of polyether 2000D.

[0068] The filler includes 15 parts of talcum powder, 10 parts of heavy calcium carbonate powder and 10 parts of ordinary Portland cement.

[0069] A method for preparing a polyurethane waterproof coating comprises the following steps:

[0070] S1 A component: put the first polyether polyol and plasticizer into a reaction kettle, raise the temperature to 60°C while stirring, add diphenylmethane diisocyanate (MDI) and stir to raise the temperature, keep the temperature at (80°C±2)°C for 2h, cool to 60°C, discharge and package.

[0071] S2 B component: weigh the second polyether polyol, Tween, plasticizer and water according to the ratio and pour them into a stirring kettle, stir for 10 minutes, add various fillers, stir for 1 hour, grind 3 times with a three-roll grinder, and then send to the stirring kettle for mixing evenly before unloading and packaging.

[0072] S3 A component: B component = 1:2 (weight ratio) stir evenly, react and solidify to form a film.

[0073] Example 2

[0074] A polyurethane waterproof coating comprises the following components:

[0075] Component A: 60 parts of a first polyether polyol, 35 parts of diphenylmethane diisocyanate and 5 parts of a synthetic plant ester plasticizer;

[0076] The 30 parts of the first polyether polyol include polyether polyol 330N, 24 parts of polyether polyol 2000D, 10 parts of polyether polyol 1000D and 4 parts of polyether polyol 400D.

[0077] Component B: 50 parts of the second polyether polyol, 32 parts of filler, 1.5 parts of pigment, 4 parts of water, 1.5 parts of catalyst, 8 parts of plasticizer, 1 part of Tween and 2 parts of thixotropic agent;

[0078] The second polyether polyol includes polyether polyol 330N, polyether polyol 2000D, polyether polyol 1000D and polyether polyol 400D.

[0079] The filler includes 12 parts of talcum powder, 10 parts of heavy calcium carbonate powder and 10 parts of ordinary Portland cement.

[0080] A method for preparing a polyurethane waterproof coating comprises the following steps:

[0081] S1 A component: put the first polyether polyol and plasticizer into a reaction kettle, raise the temperature to 60°C while stirring, add diphenylmethane diisocyanate (MDI) and stir to raise the temperature, keep the temperature at (80°C±2)°C for 2h, cool to 60°C, discharge and package.

[0082] S2 B component: weigh the second polyether polyol, Tween, plasticizer and water according to the ratio and pour them into a stirring kettle, stir for 10 minutes, add various fillers, stir for 1 hour, grind 3 times with a three-roll grinder, and then send to the stirring kettle for mixing evenly before unloading and packaging.

[0083] S3 A component: B component = 1:2 (weight ratio) stir evenly, react and solidify to form a film.

[0084] Example 3

[0085] A polyurethane waterproof coating comprises the following components:

[0086] Component A: 65 parts of a first polyether polyol, 30 parts of diphenylmethane diisocyanate and 5 parts of a synthetic plant ester plasticizer;

[0087] The 25 parts of the first polyether polyol include polyether polyol 330N, 300 parts of polyether polyol 2000D, 8 parts of polyether polyol 1000D and 3 parts of polyether polyol 400D.

[0088] Component B: 40 parts of the second polyether polyol, 4 / 3 parts of filler, 2 parts of pigment, 3 parts of water, 1 part of catalyst, 8 parts of plasticizer, 1 part of Tween and 2 parts of thixotropic agent;

[0089] The second polyether polyol includes polyether polyol 330N, polyether polyol 2000D, polyether polyol 1000D and polyether polyol 400D.

[0090] The filler includes 23 parts of talcum powder, 10 parts of heavy calcium carbonate powder and 10 parts of ordinary Portland cement.

[0091] A method for preparing a polyurethane waterproof coating comprises the following steps:

[0092] S1 A component: put the first polyether polyol and plasticizer into a reaction kettle, raise the temperature to 60°C while stirring, add diphenylmethane diisocyanate (MDI) and stir to raise the temperature, keep the temperature at (80°C±2)°C for 2h, cool to 60°C, discharge and package.

[0093] S2 B component: weigh the second polyether polyol, Tween, plasticizer and water according to the ratio and pour them into a stirring kettle, stir for 10 minutes, add various fillers, stir for 1 hour, grind 3 times with a three-roll grinder, and then send to the stirring kettle for mixing evenly before unloading and packaging.

[0094] S3 A component: B component = 1:2 (weight ratio) stir evenly, react and solidify to form a film.

[0095] Example 4

[0096] The polyurethane waterproof coating of Example 4 is mainly used for plane construction, while the polyurethane waterproof coatings of Examples 1-3 are mainly used for facade construction.

[0097] The difference between Example 4 and Example 3 is that step S3 is different. Step S3 of Example 4 is: take component A: component B = 1:2 (weight ratio), first add 3 parts of water to component B and stir component B evenly, then mix component A and component B, stir evenly, and react to solidify into a film.

[0098] Performance Test:

[0099] The polyurethane waterproof coatings of Examples 1-3 were tested, and the test results are shown in Table 2.

[0100] Table 2

[0101]

[0102]

[0103] It can be seen from Table 2 that the polyurethane waterproof coatings obtained in Examples 1-3 have excellent performance and meet national standards, such as anti-sagging properties reaching 425-764 μm.

[0104] The polyurethane waterproof coatings of Examples 1-3 were subjected to tensile strength tests. The test results are as follows: Figure 1 As shown, the polyurethane waterproof coatings of Examples 1-3 were tested for elongation at break, and the test results are shown in Figure 2 shown.

[0105] from Figure 1-2 It can be known that when MDI and polyether polyol are used to synthesize prepolymer, due to the excess of MDI, the prepolymer contains free -NCO, and the content of free -NCO is one of the most important technical parameters that determine the performance of polyurethane waterproof coatings. Specifically, Example 1 includes 20 parts of diphenylmethane diisocyanate; Example 2 includes 25 parts of diphenylmethane diisocyanate; and Example 3 includes 30 parts of diphenylmethane diisocyanate.

[0106] By changing the amount of diphenylmethane diisocyanate, the content of -NCO in the prepolymer can be changed, and then the mechanical properties of the polyurethane waterproof coating can be adjusted. The test shows that when the content of -NCO in the prepolymer (w-NCO) increases from 3.5% to 5.5%, the tensile strength and elongation at break of the coating film gradually increase. When the -NCO content increases to a certain value, the elongation at break begins to decrease. This is because as the -NCO content in the prepolymer increases, the rigid chain segments in the prepolymer increase, the polar groups increase, and it is easy to form hydrogen bonds, which increases the tensile strength of the coating film; and when the -NCO content increases to a certain value, the molecular chain of the prepolymer becomes shorter, the molecular weight decreases, and the increase in rigid groups limits the movement of the molecular chain during the stretching process, which reduces the elongation at break of the coating film. The test results show that when using MDI to produce polyurethane waterproof coatings, the -NCO content in the prepolymer should be lower than when using TDI, and should be controlled at 4.5% to 5.0%.

[0107] From the above reaction formula of diphenylmethane diisocyanate and water, it can be seen that 1 part of water can react with about 5 parts of -NCO. If the ratio of A and B components is 1:2, the -NCO content in the prepolymer is controlled at 4.5% to 5.0%, and the theoretical amount of water added in component B is less than 1%, but the actual amount of water added is far more than 1%. The amount of water added should also consider other factors. In component B, most of the water will be adsorbed by the powder filler, and the powder filler will be coated by the liquid filler. The reaction of water and prepolymer is carried out through the interface after mixing; in addition, although the boiling point of water is 100°C at normal pressure, it will still volatilize at a temperature as low as 0°C. Therefore, if the amount of water is too little, the curing time of the coating will be slowed down at low temperatures and the surface will be sticky; at high temperatures, it will cause bubbling of the coating. Although too much water can ensure that it reacts completely with -NCO, excessive water will make the coating soft, and as time goes by, water will escape from the coating to form pinholes. Therefore, the amount of water added to component B should be determined mainly based on the construction temperature, and is generally controlled at 3% to 6%.

[0108] The polyurethane waterproof coating in Example 4 was tested, and the test results are shown in Table 3.

[0109] Table 3

[0110]

[0111] The polyurethane waterproof coating of Example 4 was tested for stability: after testing, the polyurethane waterproof coating of Example 4 reached or exceeded the technical requirements of the national standard GB / T 19250-2013 "Polyurethane Waterproof Coating". The product has stable quality and a long storage period. The sealed storage period of components A and B can reach 1 year. It shows that even if 3 parts of water are added to the polyurethane waterproof coating of Example 4 to adapt to flat construction, the obtained polyurethane waterproof coating still has excellent performance and its leveling property can meet the standard.

[0112] It can be seen from Tables 2-3 that before the additional addition of 3 parts of water, the polyurethane waterproof coatings of Examples 1-3 obtained have excellent anti-sagging properties and can at least be used for facade construction; and after the additional addition of 3 parts of water, the polyurethane waterproof coating of Example 4 obtained still has good leveling properties and can at least be used for plane construction. In summary, it is shown that the polyurethane waterproof coating of the present invention is dual-purpose, that is, it can be used for plane construction and can also be used for facade construction, and is a dual-purpose environmentally friendly solvent-free two-component polyurethane waterproof coating.

[0113] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A polyurethane waterproof coating, characterized in that: The raw materials used to prepare the polyurethane waterproof coating include the following components A and B in parts by weight: The component A comprises 70-100 parts of a first polyether polyol and 20-30 parts of diphenylmethane diisocyanate; The component B comprises 45-60 parts of a second polyether polyol, 40-60 parts of a filler, 6-10 parts of water and 2-5 parts of a catalyst; The first polyether polyol and the second polyether polyol are independently selected from at least one of polyether polyol 330N, polyether polyol 2000D, polyether polyol 1000D and polyether polyol 400D; The component A further comprises 10-30 parts by weight of a plasticizer; the component B further comprises 9-20 parts by weight of a plasticizer; The filler includes at least one of silicate cement, heavy calcium carbonate powder, talcum powder and light calcium carbonate powder; Plasticizer is synthetic plant ester - environmentally friendly plasticizer.

2. A polyurethane waterproof coating according to claim 1, characterized in that: The component B also includes the following components in parts by weight: 1-5 parts of surfactant and 1-2 parts of thixotropic agent.

3. A method for preparing a polyurethane waterproof coating as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: Mixing a first polyether polyol and diphenylmethane diisocyanate, and heating to obtain the component A; Mixing a second polyether polyol, a filler, water and a catalyst to obtain the component B; The component A and the component B are mixed in a weight ratio of 1-2:2-4 to obtain the polyurethane waterproof coating.

4. The method according to claim 3, characterized in that: The heating temperature is 60-80°C.

5. The method according to claim 3, characterized in that: The following steps are also included: After heating, keep the temperature constant for 2-3 hours, then cool down to 50-60℃.