A kind of polyurea electrostatic conductive floor coating and preparation method thereof

By using a complex of conductive mica and aluminum dihydroxyglycinate combined with surfactants and small molecular weight inorganic electrolytes in polyurea coatings, the problem of poor dispersion of conductive components in polyurea coatings is solved and efficient conductive performance and stability are achieved , significantly improving the conductivity and electrostatic adsorption of the coating.

CN116694205BActive Publication Date: 2024-10-29GUANGDONG JIANPAI NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310508129.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-10-29
Estimated Expiration
2043-05-08
Patent Text Reader

Abstract

The invention discloses a polyurea electrostatic conductive floor coating and a preparation method thereof. The coating consists of a component A and a component B in a weight ratio of 1:0.5-1: the component A comprises the following components in parts by weight: 45-70 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 1-3 parts of fumed silica, 3-5 parts of a matting agent, 0.2-0.4 parts of a leveling agent, 1-2 parts of a defoaming agent, 30-35 parts of a filler, 0.2-0.4 parts of a wetting dispersant, 15-30 parts of a color paste, 10-20 parts of conductive mica, 0.5-2 parts of dihydroxyglycinate aluminum, and 1-3 parts of a conductive dispersant; the component B comprises the following components in parts by weight: 65-85 parts of a high-solid content G4899-80 elastic weather-resistant curing agent, 2-15 parts of an HDI trimer, and 10-25 parts of an aliphatic isocyanate monomer. The invention has the characteristics of low dispersion difficulty, good uniformity, high stability and strong conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wind turbine blade topcoats, and in particular to a polyurea electrostatic conductive floor coating and a preparation method thereof. Background Art

[0002] Polyurea is an elastomeric substance generated by the reaction of isocyanate components and amino compound components. Polyurea coatings have outstanding advantages such as good flexibility, no cracking, good chemical resistance, wear resistance, weather resistance, and fast curing speed. They can be widely used in waterproofing, anti-corrosion and flooring, etc.

[0003] In order to expand the application of polyurea materials in floor coatings, Chinese invention patent application CN106675485A discloses a polyurea antistatic elastic self-leveling floor coating and a preparation method thereof, which is composed of components A and B. The component A includes 5 parts of polyaspartic acid resin with an NH equivalent of 280, 40 parts of polyaspartic acid resin with an NH equivalent of 335, 0.8 parts of wetting dispersant, 0.5 parts of leveling agent, 0.3 parts of defoaming agent, 0.5 parts of fumed silica, 5 parts of rutile filler, 30.9 parts of 1250 mesh barium sulfate, 2 parts of silane coupling agent, 10 parts of color paste, and 5 parts of conductive pre-made pulp; the component B includes 95 parts of isocyanate curing agent with an NCO content of 4.9% and 5 parts of isocyanate curing agent with an NCO content of 22%. The polyurea coating of this solution has outstanding advantages such as good flexibility, no cracking, good chemical resistance, wear resistance, weather resistance, and fast curing speed. It also has excellent conductive properties and is suitable for use as floor coating in environments such as communication rooms and laboratories.

[0004] At the same time, Chinese invention patent application CN115491108A discloses an antistatic non-flammable wear-resistant polyurea floor coating and a preparation method thereof. The components of the antistatic non-flammable wear-resistant polyurea floor coating are calculated by mass percentage as follows: amino resin 15%-25%, modified acrylic resin 8%-10%, polycaprolactone polyol 20%-30%, ammonium polyphosphate 10%-16%, pentaerythritol 5%-15%, melamine 2%-4%, aluminum hydroxide 5%-8%, N, N-dimethylformamide 6%-10%, kerosene 2%-5%. The scheme can combine ammonium polyphosphate, pentaerythritol and melamine into an expansion flame retardant system by adding them, so that the coating has excellent flame retardant performance. At the same time, aluminum hydroxide is also added to the coating to further improve the overall flame retardant performance of the coating. Moreover, since aluminum hydroxide is added to the coating, the hydroxyl group of aluminum hydroxide interacts with moisture in the air through hydrogen bonds, etc., to form a conductive layer on the surface of the coating, thereby improving the overall antistatic performance of the coating.

[0005] It can be seen that the polyurea antistatic coatings of the above prior art all contain conductive components and have low resistivity, so they have the function of conducting current and removing static charges accumulated by objects. However, after adding the conductive components, there will also be dispersion problems. Taking CN106675485A as an example, the conductive pre-slurry contains 3% of nano-conductive tube additives. Even if a separate conductive pre-slurry process is set, its dispersion uniformity is still to be improved; taking CN115491108A as an example, aluminum hydroxide is added to the coating, so that the hydroxyl groups of aluminum hydroxide interact with the moisture in the air through hydrogen bonds and the like to form a conductive layer on the surface of the coating. However, it must be noted that aluminum hydroxide is an inorganic particle, and its dispersibility is actually particle dispersion. Its dispersion process mainly includes three stages: wetting, deagglomeration and stabilization of dispersed particles. In the oil phase polyurea coating system, only the oscillation process of step (3) can neither completely wet nor effectively deagglomerate, and its subsequent stabilization effect is also average. Summary of the invention

[0006] The purpose of the present invention is to provide a polyurea electrostatic conductive floor coating and a preparation method thereof, which has the characteristics of low dispersion difficulty, good uniformity, high stability and strong conductivity.

[0007] The present invention can be implemented by the following technical solutions:

[0008] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of an A component and a B component in a weight ratio of 1:0.5-1: the A component comprises the following components in parts by weight: 45-70 parts of a K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 1-3 parts of fumed silica, 3-5 parts of a matting agent, 0.2-0.4 parts of a leveling agent, 1-2 parts of a defoaming agent, 30-35 parts of a filler, 0.2-0.4 parts of a wetting dispersant, 15-30 parts of a color paste, 10-20 parts of conductive mica, 0.5-2 parts of dihydroxyglycinate aluminum, and 1-3 parts of a conductive dispersant; the B component comprises the following components in parts by weight: 65-85 parts of a high solid content G4899-80 elastic weather-resistant curing agent, 2-15 parts of an HDI trimer, and 10-25 parts of an aliphatic isocyanate monomer.

[0009] Furthermore, the conductive dispersant is a composite of a surfactant and a small molecular weight inorganic electrolyte.

[0010] Further, the low molecular weight inorganic electrolyte includes one or more of sodium silicate, sodium aluminate and / or potassium tripolyphosphate.

[0011] Furthermore, the surfactant includes one or more of stearic acid, paraffin and / or chlorinated paraffin.

[0012] Furthermore, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

[0013] Furthermore, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin.

[0014] Furthermore, the K8800 modified polyaspartic acid ester resin is a fluorine-silicon modified urea-based compound.

[0015] Furthermore, the high solid content G4899-80 elastic weather-resistant curing agent is polyester diol modified isophorone diisocyanate.

[0016] Furthermore, the NCO value of the polyester diol-modified isocyanate is 4.4-4.8%; and the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0017] Another aspect of the present invention is to protect the preparation method of the above-mentioned polyurea electrostatic conductive floor coating, comprising the following steps:

[0018] S1. Preparation of component A: Add K8800 modified polyaspartic acid ester resin into a mixing tank, start stirring at a stirring speed of 400-800r / min, then add a wetting dispersant, a leveling agent, a defoaming agent, and a matting agent into the mixing tank in sequence, stir for 15 minutes, then add fillers, conductive mica, dihydroxyglycinate aluminum, and a conductive dispersant into the mixing tank, stir for more than 30 minutes until the mixture fineness reaches 30um, and obtain component A;

[0019] S2. Preparation of component B: Add HDI trimer, G4899-80 elastic weather-resistant curing agent and aliphatic isocyanate monomer into a mixing tank, and disperse at a stirring speed of 400-800 r / min for more than 20 minutes to obtain component B;

[0020] S3. Package for standby use: Take component A and component B with a mass ratio of A:B=1:0.5-1 and package them separately.

[0021] In the present invention, K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. This component is prepared by the method of Chinese invention patent CN201811647569.1 and is produced by Guangdong Jianpai New Materials Co., Ltd. Specifically, this component is selected based on its advantages of being solvent-free and environmentally friendly. Specifically, this component is selected based on its advantages of being easy to matte, and only a small amount of matting agent needs to be added to achieve the glossiness of the coating.

[0022] In the present invention, the high solid content G4899-80 elastic weather-resistant curing agent is polyester diol modified isophorone diisocyanate, which is produced by Guangdong Jianpai New Materials Co., Ltd. Specifically, the component is selected based on its advantage of giving the coating elasticity and flexibility.

[0023] In the present invention, the NCO value of the polyester diol modified isocyanate is 4.4-4.8%. Specifically, the technical starting point for selecting this range is that its viscosity is moderate and it is convenient for subsequent construction. The aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate. Specifically, this component is selected based on its advantage of increasing the strength of the coating film.

[0024] The present invention discloses a polyurea electrostatic conductive floor coating and a preparation method thereof, which has the following beneficial effects:

[0025] First, the dispersibility is small. The present invention uses conductive mica and organic aluminum compounds as the material source of the conductive layer. The affinity between conductive mica and other organic polymers will not cause the problem of high dispersibility of carbon nanotubes, nor will it cause the poor wettability of inorganic particles such as aluminum hydroxide to affect the dispersibility.

[0026] Second, the uniformity is good. Conductive mica can be easily dispersed in the organic resin raw material. The hydroxyl group OH-, carboxylic acid group COO-, amino group NH 2 - and AL 3+ The ring structure is formed, and the end groups are adsorbed on the surface of the particles to form a double electric layer, which leads to an increase in the zeta potential, thereby effectively increasing the repulsion between inorganic particles, avoiding agglomeration between particles, and thus improving the uniformity between particles;

[0027] Third, high stability. In the present invention, a conductive dispersant is selected to assist in the dispersion of conductive mica and dihydroxyglycinate aluminum. The essence is to select a suitable dispersant to enhance the permeability of the floating body and improve its stability and thixotropy of the chemical dispersion method. Its stability has obvious advantages over the mechanical dispersion method and the ultrasonic dispersion method.

[0028] Fourth, it has strong conductivity. Conductive mica is a composite conductive material made of lightweight mica powder as the core material, and its surface is coated with chemically stable, corrosion-resistant, and highly conductive metal oxides. Dihydroxyglycinate aluminum contains rich hydroxyl-OH. Hydroxyl groups can interact with moisture in the air through hydrogen bonds to form a conductive layer on the surface of the coating. At the same time, dihydroxyglycinate aluminum also contains hydroxyl OH-, carboxylic acid group COO-, and amino NH 2 -, different groups can be combined with adjacent AL 3+ The bonding is formed to form a two-dimensional extension, thereby expanding the two-dimensional conductive network and ensuring the conductivity of the conductive layer. DETAILED DESCRIPTION

[0029] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0030] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of an A component and a B component in a weight ratio of 1:0.5-1: the A component comprises the following components in parts by weight: 45-70 parts of a K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 1-3 parts of fumed silica, 3-5 parts of a matting agent, 0.2-0.4 parts of a leveling agent, 1-2 parts of a defoaming agent, 30-35 parts of a filler, 0.2-0.4 parts of a wetting dispersant, 15-30 parts of a color paste, 10-20 parts of conductive mica, 0.5-2 parts of dihydroxyglycinate aluminum, and 1-3 parts of a conductive dispersant; the B component comprises the following components in parts by weight: 65-85 parts of a high solid content G4899-80 elastic weather-resistant curing agent, 2-15 parts of an HDI trimer, and 10-25 parts of an aliphatic isocyanate monomer.

[0031] Furthermore, the conductive dispersant is a composite of a surfactant and a small molecular weight inorganic electrolyte.

[0032] Further, the low molecular weight inorganic electrolyte includes one or more of sodium silicate, sodium aluminate and / or potassium tripolyphosphate.

[0033] Furthermore, the surfactant includes one or more of stearic acid, paraffin and / or chlorinated paraffin.

[0034] Furthermore, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

[0035] Furthermore, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin.

[0036] Furthermore, the K8800 modified polyaspartic acid ester resin is a fluorine-silicon modified urea-based compound.

[0037] Furthermore, the high solid content G4899-80 elastic weather-resistant curing agent is polyester diol modified isophorone diisocyanate.

[0038] Furthermore, the NCO value of the polyester diol-modified isocyanate is 4.4-4.8%; and the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0039] Another aspect of the present invention is to protect the preparation method of the above-mentioned polyurea electrostatic conductive floor coating, comprising the following steps:

[0040] S1. Preparation of component A: Add K8800 modified polyaspartic acid ester resin into a mixing tank, start stirring at a stirring speed of 400-800r / min, then add a wetting dispersant, a leveling agent, a defoaming agent, and a matting agent into the mixing tank in sequence, stir for 15 minutes, then add fillers, dihydroxyglycinate aluminum, and a conductive dispersant into the mixing tank, stir for more than 30 minutes until the mixture fineness reaches 30um, and obtain component A;

[0041] S2. Preparation of component B: Add HDI trimer, G4899-80 elastic weather-resistant curing agent and aliphatic isocyanate monomer into a mixing tank, and disperse at a stirring speed of 400-800 r / min for more than 20 minutes to obtain component B;

[0042] S3. Package for standby use: Take component A and component B with a mass ratio of A:B=1:0.5-1 and package them separately.

[0043] In the present invention, the specific role of low molecular weight inorganic electrolytes is: taking sodium silicate, sodium aluminate, potassium tripolyphosphate as an example, they can dissociate and induce charging, and adsorb on the surface of the powder equipment to increase the surface potential of the particles, increase the electrostatic repulsion, and improve the reliability of the slurry. Its mechanism of action is to stabilize the electrostatic resistance.

[0044] In the present invention, the role of surfactant is as follows: surfactant is composed of two parts, lipophilic group and hydrophilic group, and is a parent molecular structure, including long-chain fat, CTAB, etc. It is mainly a steric hindrance effect, and the hydrophobic chain extends into the solvent, which has a good effect on improving the rheology of the slurry.

[0045] Taking stearic acid as an example, the specific role of the conductive dispersant is as follows: one end of stearic acid is a long-chain alkyl group with hydrophilicity, and the other end is a carboxyl group with hydrophilicity. In organoaluminum compounds, its surface has active groups such as OH-, Al- -OH, and these groups can combine with stearic acid molecules in the form of chemical hydrogen bonds. This bonding method is relatively strong. Since the stearic acid molecule is large, hydrogen bonding can only occur when 0Hˉ and O atoms are close to each other. The stearic acid molecule (RC0OH) is an asymmetric structure, and only the carboxyl end can combine with the OH on the surface of the organoaluminum. -Or Al-OH forms hydrogen bonds, thereby coating the surface of the organic aluminum particles with a monomolecular layer, and achieving a dispersing effect through steric stabilization. The long chain of stearic acid molecules fully stretches in the medium, reducing the surface tension of the organic aluminum split, hindering the collision agglomeration and gravity precipitation of the particles. In addition, when anionic surfactants are adsorbed on the surface of aluminum hydroxide agglomerate particles, the particles in the agglomerate can obtain charges of the same sign, and the particles repel each other and are easily dispersed in castor oil and polymer monomers. At the same time, stearic acid molecules can also be combined in the form of physical adsorption, so that the surface of aluminum hydroxide powder changes from hydrophilic to lipophilic, has good dispersibility in polymer base materials, and reduces oil absorption.

[0046] If the sampling composite method is selected, the composite surfactant is a composite surfactant modified with stearic acid, paraffin, and chlorinated paraffin as the matrix and with straight-chain nonionic surfactants and other reagents. Long-chain and anionic surfactants stearic acid form mixed micelles in anhydrous ethanol solution, and long-chain molecules "insert" between the surface active ions of stearic acid (similar to the interaction between fatty alcohols and ionic surfactants), which weakens the electrical repulsion between the original stearic acid "ion heads", that is, the surface charge density of the micelles is reduced, and the hydrophobic interaction between the hydrocarbon chains of stearic acid makes it easier to form micelles in the mixed solution, and the critical micelle concentration is reduced. The critical micelle concentration is lower than that of a single stearic acid surfactant, and it is easier to adsorb on the surface of organic aluminum powder, so the surface activity of composite surfactant 2 is higher than that of single stearic acid. Straight-chain nonionic surfactants are more stable and more biodegradable than nonionic surfactants containing aromatic hydrocarbons, so the organic aluminum modified by composite surfactants has better dispersibility, the lowest oil absorption, and the best modification effect. This composite surfactant not only has a good modification effect on organic aluminum, but also has a good modification effect on inorganic fillers.

[0047] Example 1

[0048] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of an A component and a B component in a weight ratio of 1:1: the A component comprises the following components in parts by weight: 70 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 2 parts of fumed silica, 3 parts of a matting agent, 0.4 parts of a leveling agent, 1.5 parts of a defoaming agent, 30 parts of a filler, 0.4 parts of a wetting dispersant, 23 parts of a color paste, 20 parts of conductive mica, 0.5 parts of dihydroxyglycinate aluminum, and 3 parts of a conductive dispersant; the B component comprises the following components in parts by weight: 85 parts of a high solid content G4899-80 elastic weather-resistant curing agent, 9 parts of an HDI trimer, and 10 parts of an aliphatic isocyanate monomer.

[0049] In this embodiment, the conductive dispersant is a composite of a surfactant and a low molecular weight inorganic electrolyte. Specifically, the low molecular weight inorganic electrolyte is sodium aluminate and potassium tripolyphosphate. The surfactant is stearic acid.

[0050] In this embodiment, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and barium sulfate powder.

[0051] In this embodiment, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified urea-based compound. The high solid content G4899-80 elastic weather-resistant curing agent is a polyester diol modified isophorone diisocyanate. The NCO value of the polyester diol modified isocyanate is 4.4-4.8%; the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0052] Example 2

[0053] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of a component A and a component B in a weight ratio of 1:0.8: the component A comprises the following components in parts by weight: 58 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 1 part of fumed silica, 5 parts of a matting agent, 0.3 parts of a leveling agent, 1 part of a defoaming agent, 35 parts of a filler, 0.3 parts of a wetting dispersant, 15 parts of a color paste, 15 parts of conductive mica, 2 parts of dihydroxyglycinate aluminum, and 2 parts of a conductive dispersant; the component B comprises the following components in parts by weight: 75 parts of a high-solid G4899-80 elastic weather-resistant curing agent, 2 parts of an HDI trimer, and 25 parts of an aliphatic isocyanate monomer.

[0054] In this embodiment, the conductive dispersant is a composite of a surfactant and a small molecular weight inorganic electrolyte. Specifically, the small molecular weight inorganic electrolyte is sodium silicate. The surfactant is paraffin.

[0055] In this embodiment, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and barium sulfate powder.

[0056] In this embodiment, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified urea-based compound. The high solid content G4899-80 elastic weather-resistant curing agent is a polyester diol modified isophorone diisocyanate. The NCO value of the polyester diol modified isocyanate is 4.4-4.8%; the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0057] Example 3

[0058] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of a component A and a component B in a weight ratio of 1:0.5: the component A comprises the following components in parts by weight: 45 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 3 parts of fumed silica, 4 parts of a matting agent, 0.2 parts of a leveling agent, 2 parts of a defoaming agent, 33 parts of a filler, 0.2 parts of a wetting dispersant, 30 parts of a color paste, 10 parts of conductive mica, 1.3 parts of dihydroxyglycinate aluminum, and 1 part of a conductive dispersant; the component B comprises the following components in parts by weight: 65 parts of a high-solid content G4899-80 elastic weather-resistant curing agent, 15 parts of an HDI trimer, and 17 parts of an aliphatic isocyanate monomer.

[0059] In this embodiment, the conductive dispersant is a composite of a surfactant and a low molecular weight inorganic electrolyte. Specifically, the low molecular weight inorganic electrolyte is sodium aluminate. The surfactant is chlorinated paraffin.

[0060] In this embodiment, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

[0061] In this embodiment, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified urea-based compound. The high solid content G4899-80 elastic weather-resistant curing agent is a polyester diol modified isophorone diisocyanate. The NCO value of the polyester diol modified isocyanate is 4.4-4.8%; the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0062] Example 4

[0063] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of an A component and a B component in a weight ratio of 1:0.5-1: the A component comprises the following components in parts by weight: 50 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 2 parts of fumed silica, 4 parts of a matting agent, 0.3 parts of a leveling agent, 1.5 parts of a defoaming agent, 33 parts of a filler, 0.3 parts of a wetting dispersant, 23 parts of a color paste, 12 parts of conductive mica, 1.3 parts of dihydroxyglycinate aluminum, and 2 parts of a conductive dispersant; the B component comprises the following components in parts by weight: 75 parts of a high-solid content G4899-80 elastic weather-resistant curing agent, 10 parts of an HDI trimer, and 18 parts of an aliphatic isocyanate monomer.

[0064] In this embodiment, the conductive dispersant is a composite of a surfactant and a low molecular weight inorganic electrolyte. Specifically, the low molecular weight inorganic electrolyte is sodium silicate or sodium aluminate. The surfactant is stearic acid or paraffin.

[0065] In this embodiment, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

[0066] In this embodiment, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified urea-based compound. The high solid content G4899-80 elastic weather-resistant curing agent is a polyester diol modified isophorone diisocyanate. The NCO value of the polyester diol modified isocyanate is 4.4-4.8%; the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0067] Example 5

[0068] The invention discloses a polyurea electrostatic conductive floor coating, which is composed of a component A and a component B in a weight ratio of 1:0.5-1: the component A comprises the following components in parts by weight: 60 parts of K8800 modified polyaspartic acid ester resin with an NH equivalent of 400-410, 2 parts of fumed silica, 4 parts of a matting agent, 0.3 parts of a leveling agent, 1.5 parts of a defoaming agent, 33 parts of a filler, 0.3 parts of a wetting dispersant, 23 parts of a color paste, 17 parts of conductive mica, 1 part of dihydroxyglycinate aluminum, and 2 parts of a conductive dispersant; the component B comprises the following components in parts by weight: 75 parts of a high-solid content G4899-80 elastic weather-resistant curing agent, 8 parts of an HDI trimer, and 15 parts of an aliphatic isocyanate monomer.

[0069] In this embodiment, the conductive dispersant is a composite of a surfactant and a low molecular weight inorganic electrolyte. Specifically, the low molecular weight inorganic electrolyte includes sodium silicate, sodium aluminate and potassium tripolyphosphate. The surfactant includes stearic acid, paraffin and chlorinated paraffin.

[0070] In this embodiment, the dispersant is BYK-110, the leveling agent is TEGO-1484, the defoamer is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

[0071] In this embodiment, the K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin. The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified urea-based compound. The high solid content G4899-80 elastic weather-resistant curing agent is a polyester diol modified isophorone diisocyanate. The NCO value of the polyester diol modified isocyanate is 4.4-4.8%; the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

[0072] Example 6

[0073] Another aspect of the present invention is to protect the preparation method of the above-mentioned polyurea electrostatic conductive floor coating, comprising the following steps:

[0074] S1. Preparation of component A: Add K8800 modified polyaspartic acid ester resin into a mixing tank, start stirring at a stirring speed of 400-800r / min, then add a wetting dispersant, a leveling agent, a defoaming agent, and a matting agent into the mixing tank in sequence, stir for 15 minutes, then add fillers, conductive mica, dihydroxyglycinate aluminum, and a conductive dispersant into the mixing tank, stir for more than 30 minutes until the mixture fineness reaches 30um, and obtain component A;

[0075] S2. Preparation of component B: Add HDI trimer, G4899-80 elastic weather-resistant curing agent and aliphatic isocyanate monomer into a mixing tank, and disperse at a stirring speed of 400-800 r / min for more than 20 minutes to obtain component B;

[0076] S3. Package for standby use: Take component A and component B with a mass ratio of A:B=1:0.5-1 and package them separately.

[0077] In order to verify the performance of the product of the present invention, Examples 1-3 were prepared respectively by the preparation method of Example 6, and then sprayed by the method of Example 6, and then relevant performance tests were performed. The specific test results are shown in the following table:

[0078] Table 1 Performance test results

[0079] Serial number Project Name Technical indicators Example 1 Example 2 Example 3 Example 4 1 Surface resistance ≥104Ω·cm-2 ≤1011Ω·cm-2 5*107Ω·cm-2 6*107Ω·cm-2 8*107Ω·cm-2 4*106Ω·cm-2 2 Electrostatic adsorption force on coating surface ≥9.0KN / m 9.6 9.5 9.7 10.3

[0080] The above embodiments are only specific embodiments of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.

Claims

1. A polyurea electrostatic conductive floor coating, Features It is composed of component A and component B in a weight ratio of 1:0.5-1: The component A comprises the following components by weight: 45-70 parts of K8800 modified polyaspartic acid ester resin with NH equivalent of 400-410, 1-3 parts of fumed silica, 3-5 parts of matting agent, 0.2-0.4 parts of leveling agent, 1-2 parts of defoaming agent, 30-35 parts of filler, 0.2-0.4 parts of wetting dispersant, 15-30 parts of color paste, 10-20 parts of conductive mica, 0.5-2 parts of dihydroxyglycinate aluminum, and 1-3 parts of conductive dispersant; The B component includes the following components in parts by weight: 65-85 parts of high solid content G4899-80 elastic weather-resistant curing agent, 2-15 parts of HDI trimer, and 10-25 parts of aliphatic isocyanate monomer; The conductive dispersant is a complex of a surfactant and a low molecular weight inorganic electrolyte; the low molecular weight inorganic electrolyte includes one or more of sodium silicate, sodium aluminate and / or potassium tripolyphosphate; the surfactant includes one or more of stearic acid and paraffin.

2. The polyurea electrostatic conductive floor coating according to claim 1, Features: The wetting and dispersing agent is BYK-110, the leveling agent is TEGO-1484, the defoaming agent is TEGO-900, and the filler is rutile titanium dioxide and / or barium sulfate powder.

3. The polyurea electrostatic conductive floor coating according to claim 2, Features: The K8800 modified polyaspartic acid ester resin is a fluorosilicone modified aliphatic diamine resin.

4. The polyurea electrostatic conductive floor coating according to claim 3, Features: The K8800 modified polyaspartic acid ester resin is a fluorine-silicon modified urea-based compound.

5. The polyurea electrostatic conductive floor coating according to claim 4, Features: The high solid content G4899-80 elastic weather-resistant curing agent is polyester diol modified isophorone diisocyanate.

6. The polyurea electrostatic conductive floor coating according to claim 5, Features: The NCO value of the polyester diol-modified isophorone diisocyanate is 4.4-4.8%; and the aliphatic isocyanate monomer is hydrogenated diphenylmethane diisocyanate.

7. A method for preparing the polyurea electrostatic conductive floor coating according to any one of claims 1 to 6, Features The following steps are involved: S1. Preparation of component A: Add K8800 modified polyaspartic acid ester resin into a mixing tank, start stirring at a stirring speed of 400-800 r / min, then add a wetting dispersant, a leveling agent, a defoaming agent, and a matting agent into the mixing tank in sequence, stir for 15 minutes, then add fillers, conductive mica, dihydroxyglycinate aluminum, and a conductive dispersant into the mixing tank, stir for more than 30 minutes until the mixture has a fineness of 30 μm, and obtain component A; S2. Preparation of component B: Add HDI trimer, G4899-80 elastic weather-resistant curing agent and aliphatic isocyanate monomer into a mixing tank, and disperse at a stirring speed of 400-800 r / min for more than 20 minutes to obtain component B; S3. Package for standby use: Take component A and component B with a mass ratio of A:B=1:0.5-1 and package them separately.

Citation Information

Patent Citations

  • Polyurea anti-static elastic self-leveling floor coating and preparation method thereof

    CN106675485A

  • A method for preparing a fluorosilicone-modified urea compound

    CN109851738B

  • Anti-static, misfire and wear-resistant polyurea floor coating and preparation method thereof

    CN115491108A

  • Anticorrosive static-conductive solvent-free polyurea coating as well as preparation method and application thereof

    CN114149729A

  • Environment-friendly wind power blade finish paint as well as preparation method and use method thereof

    CN114316763A