A honeycomb CO oxidation catalyst carrier material and preparation method thereof

By applying a combination material of honeycomb metal oxide composite support and palladium metal coating in the steel industry, the problem of insufficient efficiency and sulfur resistance of existing catalysts in high humidity flue gas and high sulfur dioxide environments is solved, and high efficiency CO is achieved Oxidation and long-lived catalysts that support the recycling of palladium metals.

CN116712996BActive Publication Date: 2024-11-08CECEP LIUHE TIANRONG (SHANDONG) CATALYST CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310494685.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-08
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

The existing honeycomb CO oxidation catalysts are limited in applications in sintering machines and steel rolling heating furnaces in the steel industry, especially in high-humidity flue gas and high sulfur dioxide environments. The catalytic efficiency and sulfur resistance are insufficient, making it difficult to meet the industry's needs.

Method used

A combination material of honeycomb metal oxide composite support and palladium metal coating is used, with specific components of 80-85% TiO2, 3-6% WO3, 0.3-0.5% V2O5, and the balance is Al2O3 and SiO2, and it is impregnated. The coating method is supported by palladium metal to prepare an efficient CO oxidation catalyst support material.

Benefits of technology

It achieves high oxidation efficiency (up to 90%), high aerial speed (15000~20000h-1), low acting temperature and good sulfur resistance, extends the service life of the catalyst to at least 2 years, and supports the recycling of precious metal palladium, reducing pollutant emissions and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004211511030000071
    Figure BDA0004211511030000071
  • Figure BDA0004211511030000072
    Figure BDA0004211511030000072
  • Figure BDA0004211511030000081
    Figure BDA0004211511030000081
Patent Text Reader

Abstract

The present invention relates to the technical field of carbon monoxide catalytic oxidation, and in particular, to a honeycomb CO oxidation catalyst carrier material and a preparation method thereof. The material comprises a honeycomb metal oxide composite carrier and a palladium metal coating loaded on the surface of the honeycomb metal oxide composite carrier; the components of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 80-85% TiO2, 3-6% WO3, 0.3-0.5% V2O5, and the remainder is Al2O3 and SiO2. The catalyst carrier material uses transition metals and precious metal palladium as catalytic components; it has the characteristics of high oxidation efficiency, high air velocity and low action temperature; it also has the advantages of high catalytic activity, high CO oxidation efficiency, extremely low catalyst activity decay rate and stable performance; it is suitable for high-humidity flue gas conditions and working conditions after flue gas desulfurization; the preparation method has low cost, good effect and high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon monoxide catalytic oxidation, and in particular to a honeycomb CO oxidation catalyst carrier material and a preparation method thereof. Background Art

[0002] Existing CO catalysts are mostly used in the petrochemical, waste incineration, and automobile exhaust industries.

[0003] Honeycomb CO oxidation catalysts use metal oxide composite carriers. Metal oxides are mostly CuO-CeO2 and Al2O3 as the main materials, and transition metals and precious metals platinum are used as catalytic components. Honeycomb CO oxidation catalysts have the characteristics of high oxidation efficiency, high space velocity and low action temperature. Honeycomb CO oxidation catalysts with CuO-CeO2 as the main material are mostly used in the chemical industry. Honeycomb CO oxidation catalysts with Al2O3 as the main material have poor sulfur resistance. Generally, after 2 months of use, the CO oxidation performance decreases significantly.

[0004] At present, there is no honeycomb CO oxidation catalyst that can be particularly used in sintering machines and steel rolling heating furnaces in the steel industry. This is mainly because higher CO catalytic efficiency is required in sintering machines and steel rolling heating furnaces in the steel industry, and the sulfur dioxide content in the flue gas in this field is relatively high. The above-mentioned prior art honeycomb CO oxidation catalyst with CuO-CeO2 and Al2O3 as the main material loaded with precious metal palladium has poor sulfur dioxide resistance and is difficult to apply. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a honeycomb CO oxidation catalyst carrier material and a preparation method thereof.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] The present invention discloses a honeycomb CO oxidation catalyst carrier material, comprising a honeycomb metal oxide composite carrier and a palladium metal coating loaded on the surface of the honeycomb metal oxide composite carrier; the components of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 80-85% TiO2, 3-6% WO3, 0.3-0.5% V2O5, and the remainder is Al2O3 and SiO2.

[0008] Furthermore, the loading depth of the palladium metal coating is 1.5 to 3 mm.

[0009] Furthermore, the composition of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 82% TiO2, 4% WO3, 0.4% V2O5, and the remainder is Al2O3 and SiO2.

[0010] The present invention also provides a method for preparing the above-mentioned honeycomb CO oxidation catalyst carrier material, comprising the following steps:

[0011] S1, preparing an initial dry embryo module of the honeycomb metal oxide composite carrier;

[0012] S2, dipping the initial dry embryo module into a palladium salt solution for the first time;

[0013] S3, drying the dried embryo module after the first dipping;

[0014] S4, dipping the dried embryo module obtained in step S3 for a second time;

[0015] S5, sequentially drying and calcining the dry embryo module after the second impregnation to obtain the honeycomb CO oxidation catalyst carrier material.

[0016] Furthermore, the module specific pore volume of the initial dry embryo module is 0.2 to 0.25 cm 3 / g.

[0017] Furthermore, in step S2, the palladium salt solution used for the first impregnation is a palladium nitrate solution with a mass percentage of 2.5% to 3.4% and a pH value of 2 to 3; relative to the initial dry embryo module, the mass of the dry embryo module after the first impregnation increases by 28% to 34%.

[0018] Furthermore, in step S3, the drying temperature is 50-60° C., and the drying time is 48-60 hours.

[0019] Furthermore, in step S4, the palladium salt solution used for the second impregnation is a palladium nitrate solution with a mass percentage of 1.2‰ to 1.7‰ and a pH value of 1.5 to 2.5; relative to the dry embryo module obtained in step S3, the mass of the dry embryo module after the second impregnation increases by 15% to 23%.

[0020] Furthermore, in step S5, the drying temperature is 50-60° C., the drying time is 72 hours, and the calcination activation temperature is 520-560° C., and the time is 6-8 hours.

[0021] Furthermore, in step S1, the preparation method of the initial dry embryo module is: mixing raw materials according to the mass percentage of each component in the honeycomb metal oxide composite carrier, adding deionized water and stirring evenly; adjusting the pH to 2-4, standing for 24 hours, and then filtering, extruding, cutting, drying, calcining and cooling to obtain the initial dry embryo module.

[0022] The beneficial effects of the present invention are:

[0023] (1) The honeycomb-shaped CO oxidation catalyst carrier material of the present invention uses transition metal and precious metal palladium as catalytic components, and has the characteristics of high oxidation efficiency, high space velocity and low action temperature. The oxidation efficiency reaches 90%, and the volume space velocity can reach 15000-20000h -1 ;

[0024] (2) The honeycomb-shaped CO oxidation catalyst carrier material of the present invention, the components of the honeycomb metal oxide composite carrier are TiO2, WO3, V2O 5、 Al2O3 and SiO2 make the catalyst carrier material have the advantages of high catalytic activity, high CO oxidation efficiency, extremely low catalyst activity decay rate and stable performance;

[0025] (3) The honeycomb CO oxidation catalyst carrier material of the present invention is suitable for high-humidity flue gas conditions and post-flue gas desulfurization working conditions;

[0026] (4) The honeycomb CO oxidation catalyst carrier material of the present invention has a service life of at least 2 years under the same conditions; after the chemical performance fails, the precious metal palladium in the waste catalyst can be recovered and reused, thereby reducing pollutant emissions and saving costs;

[0027] (5) The method for preparing the honeycomb CO oxidation catalyst carrier material of the present invention adopts an immersion coating method to load palladium metal, which has low preparation cost, good effect and high efficiency. DETAILED DESCRIPTION

[0028] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0029] The honeycomb CO oxidation catalyst carrier material of the present invention comprises a honeycomb metal oxide composite carrier and a palladium metal coating loaded on the surface of the honeycomb metal oxide composite carrier; the components of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 80-85% TiO2, 3-6% WO3, 0.3-0.5% V2O5, and the remainder is Al2O3 and SiO2.

[0030] The honeycomb CO oxidation catalyst carrier material of the present invention uses transition metal and noble metal palladium as catalytic components, has the characteristics of high oxidation efficiency, high space velocity and low action temperature, the oxidation efficiency reaches 90%, and the volume space velocity can reach 15000-20000h -1 The catalyst material has good anti-sulfur performance, high catalytic activity, high CO oxidation efficiency, extremely low catalyst activity decay rate and stable performance, making it more suitable for use in the steel industry sintering machine and steel rolling heating furnace industry under high humidity flue gas conditions and post-flue gas desulfurization working conditions.

[0031] Preferably, in the honeycomb CO oxidation catalyst carrier material of the present invention, the loading depth of the palladium metal coating is 1.5 to 3 mm.

[0032] Preferably, the loading depth of the palladium metal coating is 2 mm.

[0033] Preferably, the composition of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 82% TiO2, 4% WO3, 0.4% V2O5, and the remainder is Al2O3 and SiO2.

[0034] The method for preparing the honeycomb CO oxidation catalyst carrier material of the present invention comprises the following steps:

[0035] S1, preparing an initial dry embryo module of a honeycomb metal oxide composite carrier;

[0036] S2, dipping the initial dry embryo module into a palladium salt solution for the first time;

[0037] S3, drying the dried embryo module after the first dipping;

[0038] S4, dipping the dried embryo module obtained in step S3 for a second time;

[0039] S5. The dried embryo module after the second impregnation is sequentially dried and calcined to activate, so as to obtain a honeycomb CO oxidation catalyst carrier material.

[0040] In the above preparation method of the present invention, the initial dry embryo module is immersed in a palladium salt solution twice, so that the palladium metal can be evenly distributed in the honeycomb metal oxide composite carrier. At the same time, the number of immersion times is small and the production cost is low.

[0041] Specifically, when preparing honeycomb CO oxidation catalyst carrier materials, one of the important steps to determine its oxidation efficiency and effect is to control the liquid absorption of the dry embryo module. The dry embryo module is required to have a suitable particle shape, uniform particle size, uniform particle distribution, and a specific surface area range of 660-690m 2 / m 3 , the pore size range is 4 to 6 mm. It also needs to have sufficient water absorption, which is obtained by immersing the dry embryo in water and conducting a water absorption test, with a water absorption weight ratio of 28 to 34%. In addition, the dry embryo module also needs to not chemically react with the impregnation solution. For the palladium salt impregnation solution, its concentration and pH value are also important. The amount of impregnation solution absorbed by the dry embryo module depends on its specific pore volume and the concentration of the impregnation solution.

[0042] Preferably, the specific surface area of ​​the dry embryo module is 688m 2 / m 3 , the aperture is 4.5mm.

[0043] Preferably, the module specific pore volume of the initial dry embryo module of the present invention is 0.2 to 0.25 cm 3 / h.

[0044] Preferably, in the above-mentioned preparation method of the present invention, in step S2, the palladium salt solution used for the first impregnation is a palladium nitrate solution with a mass percentage of 2.5% to 3.4% and a pH value of 2 to 3; relative to the initial dry embryo module, the mass of the dry embryo module after the first impregnation increases by 28% to 34%.

[0045] Further preferably, the mass percentage of the palladium nitrate solution is 3%, and the mass of the dry embryo module is increased by 30%.

[0046] Preferably, the first immersion time in step S2 is 10 to 20 minutes; the immersion time can achieve a 30% weight increase in the dry embryo module.

[0047] Preferably, in step S3, the drying temperature is 50-60° C., and the drying time is 48 to 60 hours.

[0048] Preferably, in step S4, the palladium salt solution used for the second impregnation is a palladium nitrate solution with a mass percentage of 1.2‰ to 1.7‰ and a pH value of 1.5 to 2.5; relative to the dry embryo module obtained in step S3, the mass of the dry embryo module after the second impregnation increases by 15% to 23%.

[0049] Further preferably, the mass percentage of the palladium nitrate solution is 1.5‰, and the mass of the dry embryo module increases by 20%.

[0050] Preferably, in step S4, the second immersion time is 15 min; the immersion time can achieve the dry embryo module to increase weight by 20% again.

[0051] Preferably, in step S5, the drying temperature is 50-60°C, and the drying time is 72 hours; the calcination activation temperature is 520-560°C, preferably 550°C; and the calcination activation time is 6-8 hours, preferably 6 hours.

[0052] Preferably, in step S1, the preparation method of the initial dry embryo module is: mixing the raw materials according to the mass percentage of each component in the honeycomb metal oxide composite carrier, adding deionized water and stirring evenly; adjusting the pH to 2-4 and then fermenting; filtering, extruding, cutting, and then drying, calcining and cooling to obtain the initial dry embryo module.

[0053] Further preferably, the preparation method of the initial dry embryo module is: after mixing the raw materials, add deionized water and stir evenly, use ammonia water to adjust the pH for 4 to 6 hours to obtain wet material, "ferment" the wet material for 24 hours, and then filter to obtain the embryo material. The "fermentation" referred to in this step is specifically a static process, which does not require heating or cooling and can be carried out at room temperature.

[0054] The blank is extruded into a honeycomb shape through a fixed mold and then cut to a fixed length as needed.

[0055] After cutting, the embryos are sent to the primary drying room for the first drying. During the first drying, the temperature rises from room temperature to 60°C, and the drying time is 11 days. Then they are transferred to the secondary drying room for the second drying, the temperature is 57-60°C, and the drying time is 7-10 days.

[0056] After drying, calcination is performed, and the calcination temperature is raised from room temperature to 500°C. After being kept at this temperature for 6 hours, it is naturally cooled. The natural cooling time is 28 to 40 hours to obtain an initial dry embryo module.

[0057] In addition, it is necessary to flatten the end of the initial dry embryo module according to the designed length, and then apply curing liquid to the air inlet end to harden it.

[0058] The effects of the present invention are illustrated below by means of specific embodiments.

[0059] Example

[0060] The honeycomb CO oxidation catalyst carrier material of this embodiment has a mass of 500 kg for the honeycomb metal oxide composite carrier, wherein the masses of the components are 410 kg of TiO2, 20 kg of WO3, 2 kg of V2O5, and the remainder is Al2O3 and SiO2.

[0061] In this embodiment, the thickness of the palladium metal coating layer supported on the surface of the honeycomb-shaped metal oxide composite carrier is 2 mm.

[0062] The performance test was conducted on the honeycomb CO oxidation catalyst support material of this embodiment, and the specific experimental process and results are as follows:

[0063] (1) Determination of CO oxidation efficiency

[0064] The CO oxidation efficiency of the honeycomb CO oxidation catalyst support material of this embodiment was measured in the approximate temperature range of 200-290° C. In general, as the reaction temperature increases, the CO oxidation efficiency also gradually increases. This shows that the CO oxidation efficiency of the honeycomb CO oxidation catalyst support material of this embodiment is approximately linearly related to the reaction temperature.

[0065] The specific measurement results are shown in Table 1 and Table 2, where Table 1 is the test data under laboratory conditions and Table 2 is the actual test data in the sintering machine flue gas desulfurization and denitrification project.

[0066] When the CO catalytic efficiency is tested under experimental conditions, the reaction temperature is relatively low due to the obvious heat loss during the test. However, the change trend of the CO catalytic efficiency is still gradually increasing with the increase of the reaction temperature.

[0067] Table 1 Test data under test conditions

[0068]

[0069] In addition, the present invention also tests the CO catalytic efficiency in the actual sintering machine flue gas desulfurization and denitrification project. In actual use, the sintering machine can maintain a higher reaction temperature, so the CO catalytic oxidation efficiency is higher than that of the experimental conditions.

[0070] Table 2 Actual application project data

[0071]

[0072]

[0073] It can be seen from the above table that in actual use, the CO catalytic oxidation efficiency can reach up to 73.8%.

[0074] (2) Effect of SO2 on CO oxidation efficiency

[0075] When SO2 was introduced into the experimental gas, the CO oxidation efficiency dropped immediately. After 24 hours of introduction, the SO2 was cut off and the catalyst oxidation efficiency did not recover. The poisoning effect of SO2 on the CO oxidation catalyst was significant and irreversible.

[0076] (3) Effect of NH3 on CO oxidation efficiency

[0077] When NH3 was introduced into the experimental gas, the CO oxidation efficiency decreased immediately. When the NH3 concentration increased from 15ppm to 50ppm, the CO oxidation efficiency continued to decrease. When the NH3 concentration decreased from 50ppm until the introduction was stopped, the CO oxidation efficiency recovered, indicating that the CO catalyst was affected by the NH3 concentration.

[0078] The above experimental results show that reaction temperature, SO2 concentration and NH3 concentration have an impact on the CO catalyst oxidation efficiency. The installation position of the CO oxidation catalyst is selected according to the experimental results. The CO catalyst must be installed after flue gas desulfurization and denitrification.

[0079] Honeycomb CO oxidation catalyst materials are used in sintering machines and steel rolling heating furnaces in the steel industry, and work synergistically with SCR denitrification catalysts. The honeycomb CO oxidation catalyst is filled at the end of the SCR reactor to reduce the heat load of the hot blast furnace in the desulfurization and denitrification project and reduce the CO emission concentration in the flue gas.

[0080] In addition, after the chemical properties of the honeycomb CO oxidation catalyst material of this embodiment become ineffective, the precious metal palladium in the waste catalyst can be recovered and reused, thereby reducing pollutant emissions and saving costs.

[0081] Comparative Example

[0082] The traditional honeycomb CO oxidation catalyst material is based on aluminum oxide and loaded with platinum metal. Compared with the honeycomb CO oxidation catalyst material of the embodiment of the present invention, under the same conditions, when initially used at a temperature of about 290°C, the carbon monoxide oxidation efficiency of this catalyst material is 40%. After 2 months of use, the catalyst's CO oxidation efficiency is only 19%.

[0083] The service life of the honeycomb CO oxidation catalyst material in the embodiment of the present invention in the sintering machine flue gas desulfurization and denitrification project can reach two years, and the sulfur dioxide content in the sintering machine flue gas desulfurization and denitrification project is obviously higher than the sulfur dioxide residue in the chemical industry. Therefore, there is no need for a specific separate comparison to prove that the effect of the honeycomb CO oxidation catalyst material of the present invention is better than that of the traditional platinum metal-loaded honeycomb CO oxidation catalyst.

[0084] In the description of the present invention, it should be noted that the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0085] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a honeycomb CO oxidation catalyst carrier material, characterized in that: The honeycomb CO oxidation catalyst carrier material is composed of a honeycomb metal oxide composite carrier and a palladium metal coating loaded on the surface of the honeycomb metal oxide composite carrier; the components of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 80-85% TiO2, 3-6% WO3, 0.3-0.5% V2O5, and the balance is Al2O3 and SiO2; The following steps are involved: S1, preparing an initial dry embryo module of the honeycomb metal oxide composite carrier; S2, dipping the initial dry embryo module into a palladium salt solution for the first time; S3, drying the dried embryo module after the first dipping; S4, dipping the dried embryo module for the second time; S5, sequentially drying and calcining the dry embryo module after the second impregnation to obtain the honeycomb CO oxidation catalyst support material; In the step S2, the palladium salt solution used for the first impregnation is a palladium nitrate solution with a mass percentage of 2.5% to 3.4% and a pH value of 2 to 3; the mass of the dry embryo module after the first impregnation increases by 28% to 34% relative to the initial dry embryo module; In step S4, the palladium salt solution used for the second impregnation is a palladium nitrate solution with a mass percentage of 1.2‰ to 1.7‰ and a pH value of 1.5 to 2.5; relative to the dry embryo module obtained in step S3, the mass of the dry embryo module after the second impregnation increases by 15% to 23%.

2. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: The module specific pore volume of the initial dry embryo module is 0.2 to 0.25 cm 3 / g.

3. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: In step S3, the drying temperature is 50-60° C. and the drying time is 48-60 hours.

4. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: In the step S5, the drying temperature is 50-60° C., the drying time is 72 hours, and the calcination activation temperature is 520-560° C., and the time is 6-8 hours.

5. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: In the step S1, the preparation method of the initial dry embryo module is: mixing raw materials according to the mass percentage of each component in the honeycomb metal oxide composite carrier, adding deionized water and stirring evenly; adjusting the pH to 2-4, standing for 24 hours, and then filtering, extruding, cutting, drying, calcining and cooling to obtain the initial dry embryo module.

6. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: The loading depth of the palladium metal coating is 1.5 to 3 mm.

7. The method for preparing a honeycomb CO oxidation catalyst support material according to claim 1, characterized in that: The composition of the honeycomb metal oxide composite carrier and the mass percentage of each component are: 82% TiO2, 4% WO3, 0.4% V2O5, and the remainder is Al2O3 and SiO2.

Citation Information

Patent Citations

  • Oxidation catalyst for purifying tail gas of diesel vehicles and preparation method thereof

    CN101530787A

  • Integral dioxin removing catalyst and preparation method thereof

    CN103657638A

  • Honeycomb structure and catalyst body comprising the same

    JP2009236067A

  • Sorptive catalyst for the sorptive and oxidative cleaning of exhaust gases from diesel engines

    US5591414A