A modified battery separator and its preparation method and application
By using the atomic layer deposition method to construct the conductive ion layer and the modified layer on the surface of the lithium-ion battery separator, the problem of thermal shrinkage of the separator and insufficient electrolyte wetting at high temperatures is solved, and the performance and safety of the battery are improved.
Patent Information
- Application Number
- CN202310578074.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-19
AI Technical Summary
The existing lithium-ion battery separators will experience heat shrinkage at high temperatures, increasing the risk of positive and negative electrode contact, and the non-polar surface is not conducive to electrolyte infiltration and lithium ion transmission, resulting in a decrease in ion conductivity, and the thickness of traditional ceramic film coating is too thick. Battery performance.
The nano-order conductive ion layer and modification layer are constructed on the surface of the membrane by atomic layer deposition method, which improves the ion conduction performance of the membrane, improves the electrolyte wetting property, and enhances the corrosion resistance and thermal stability of the membrane.
The uniform lithium ion distribution of the separator is achieved, the interface impedance is reduced, the coulomb efficiency and energy density of the battery are improved, while the corrosion of electrodes and separators is reduced, and the mechanical properties and thermal stability of the separator are improved.
Smart Images

Figure BDA0004243550180000121 
Figure BDA0004243550180000131 
Figure HDA0004243550190000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified battery separators, and in particular relates to a preparation method of a modified battery separator and application thereof. Background Art
[0002] The diaphragm is a key internal component of lithium-ion batteries. Its main function is to separate the positive and negative electrodes of lithium-ion batteries, keep lithium ions from passing through, and prevent short circuits due to physical contact between the two electrodes. Currently, commercially mature diaphragm materials are generally high-strength thin-film polyolefin porous membranes, such as the common polyethylene (PE) porous membrane. Diaphragm materials represented by PE membranes will undergo severe thermal shrinkage at high temperatures, thereby increasing the risk of direct contact between the positive and negative electrodes, which is a safety hazard that affects the normal use of power batteries. In addition, the non-polar surface of the diaphragm is not conducive to electrolyte infiltration and lithium ion transmission, resulting in reduced ion conductivity. To solve the above problems, people have developed a thin film coating method to improve the performance of the diaphragm, but the ceramic thin film coating manufactured by traditional methods is generally as thick as 2-5μm, which seriously compresses the available space inside the lithium battery and reduces the energy density of the lithium battery.
[0003] Therefore, it is imperative to develop a modified battery separator that can improve the mechanical properties of the separator while avoiding the impact on battery performance due to excessive coating thickness. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a modified battery separator and a preparation method and application thereof. In view of the defects of the prior art, a modified battery separator having a conductive ion layer and a modified layer of only nanometer scale is constructed on the surface of the separator by atomic layer deposition, which greatly reduces the thickness of the coating and makes the modified battery separator have the properties of high voltage resistance, ion conductivity, electrolyte affinity and corrosion resistance.
[0005] According to an embodiment of the first aspect of the present invention, a modified battery separator is provided, the battery separator comprising:
[0006] a diaphragm; a hole in the diaphragm;
[0007] Conductive ion layer; the conductive ion layer is arranged on the outer surface of the diaphragm layer;
[0008] A modified layer; the modified layer is disposed on the outer surface of the conductive ion layer;
[0009] The raw material for preparing the conductive ion layer is at least one of oxide 1 and a solid electrolyte;
[0010] The raw material for preparing the modified layer includes at least one of oxide 2, nitride and fluoride;
[0011] The conductive ion layer and the modified layer are sequentially disposed on the diaphragm by atomic layer deposition.
[0012] The embodiments according to the first aspect of the present invention have at least the following beneficial effects:
[0013] 1. The present invention uses atomic layer deposition (ALD) to precisely control the thickness and composition of the thin film coating at the atomic scale. The growth mechanism of atomic layer deposition is based on the chemical adsorption of a single atomic layer on the surface of the material, and a very thin and dense thin film material can be deposited on the inner pores and outer surface of the diaphragm at the same time. A modified battery diaphragm with a conductive ion layer and a modified layer of only nanometer-scale coating is constructed on the surface of the diaphragm by atomic layer deposition.
[0014] 2. Since the diaphragm itself does not have the ability to conduct ions and the base membrane of the diaphragm is a porous structure, the phenomenon of uneven distribution of ions on the surface of the base membrane is obvious. Lithium ions gather near the holes and are sparsely distributed far away from the holes, which leads to uneven SEI formation and increases the rupture and decomposition of the SEI layer during the cycle, thereby causing an increase in the side reactions between the active material and the electrolyte and reducing the coulombic efficiency of the battery. Therefore, a layer of ion conduction is deposited on the surface of the diaphragm. The conductive ion layer of the present invention is a conductive ion layer that has the ability to conduct ions after lithium is deintercalated or has the ability to conduct ions itself, which can significantly improve the uniformity of the distribution of lithium ions on the surface of the diaphragm, especially the ability of the diaphragm skeleton to conduct ions, which is conducive to the formation of a uniform SEI layer and reduces the interface impedance.
[0015] 3. Due to the hydrophobicity of the diaphragm, the electrolyte has poor wettability on the diaphragm. In order to improve the wettability of the diaphragm to the electrolyte and shorten the injection and standing time of the soft-pack battery, the present invention constructs a modified layer on the surface of the diaphragm skeleton through the ALD technology, which is beneficial to improve the affinity of the inside of the diaphragm to the electrolyte. Therefore, the ALD technology can simultaneously improve the wettability of the electrolyte on the surface and inside of the diaphragm. At the same time, in an electrolyte containing fluorine-containing lithium salts, HF gas is released during the cycle of the battery, which will cause corrosion to the electrode. Constructing a modified layer on the surface of the diaphragm can effectively absorb or block the corrosive gas released from the electrolyte, thereby correspondingly reducing the corrosion and damage to the electrode or diaphragm. At the same time, the modified layer of this insulating inorganic ceramic material constructed on the surface of the diaphragm skeleton can significantly improve the breakdown voltage and thermal stability of the diaphragm. Provide a new solution for manufacturing low-cost, high-energy-density and high-performance diaphragms.
[0016] In the present invention, the conductive ion layer is disposed on the outer surface of the diaphragm layer, which means that the conductive ion layer is also deposited in the holes on the diaphragm surface to significantly improve the uniformity of the distribution of lithium ions on the diaphragm surface.
[0017] According to some embodiments of the present invention, the thickness of the conductive ion layer is 0.1-20 nm.
[0018] According to some embodiments of the present invention, the thickness of the modification layer is 0.1-20 nm.
[0019] According to some embodiments of the present invention, the general chemical formula of the oxide 1 is MOx, wherein M is at least one of Ti, Al, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Ru, La, Ce, Hf, Ta, W, Mg, In, Sn and Si, and 1≤x≤5.
[0020] According to some embodiments of the present invention, the solid electrolyte includes Li x A3B2O 12 Wherein A is at least one of Y, Pr, Nd, and La, wherein B is at least one of Te, Nb, Ta, Sb, Zr, Sn, and Hf; 1≤x≤7, lanthanum titanate lithium (Li x La y Ti z O,x+3y+4z=2), lithium aluminate (Li x Al y O, x+3y=2), lithium silicate (Li x Si y O,x+4y=2), lithium tantalate (Li x Ta y O,x+5y=2), lithium niobate (Li x Nb y O, x+5y=2), lithium oxide Li2O, lithium aluminum silicate (Li x Al y Si z O,x+3y+4z=2), lithium phosphate (Li3PO4), lithium nitride (Li3N), lithium oxyphosphide (LiPON), lithium aluminum sulfide (Li x Al y S, x+3y=2) and at least one of lithium tetrafluoroaluminate (LiAlF4).
[0021] According to some embodiments of the present invention, the Li x A3B2O 12 It is a garnet-type lithium ion conductor.
[0022] According to some embodiments of the present invention, the general chemical formula of the oxide 2 is MOx, wherein M is at least one of Al, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Ru, La, Ce, Hf, Ta, W, Mg, In and Sn, and 1≤x≤5.
[0023] According to some embodiments of the present invention, the general formula of the nitride is DxNy, D is one of Al, Si, B, P, Li, Zr, 1≤x≤3, 1≤y≤5.
[0024] According to some embodiments of the present invention, the fluoride has the general formula AF x , A is one of Li, Al, Sc, Zr, La, Sm, Ce and Bi, 1≤x≤4.
[0025] According to some embodiments of the present invention, the separator includes at least one of a polyethylene separator, a polypropylene separator, a polyethylene and polypropylene multilayer separator, a Celgard separator, and a polyimide separator.
[0026] According to some preferred embodiments of the present invention, the modified battery separator includes a laminated modified battery separator;
[0027] The laminated modified battery separator comprises:
[0028] A base body; there are holes in the base body;
[0029] A multifunctional layer; the multifunctional layer is arranged on the outer surface of the substrate;
[0030] The multifunctional layer comprises a conductive ion layer and a modified layer which are sequentially stacked starting from the substrate;
[0031] The number of cycles of sequentially stacking the conductive ion layer and the modified layer is 1 or more times, for example, 1 time, 2 times or 3 times.
[0032] According to an embodiment of the second aspect of the present invention, a method for preparing the above-mentioned modified battery separator is provided.
[0033] The method comprises: placing the diaphragm into an atomic layer deposition device, and performing cyclic deposition to obtain a modified battery diaphragm with a conductive ion layer and a modification layer deposited on the outer surface of the diaphragm layer.
[0034] The preparation method of the modified battery separator,
[0035] The method comprises: S1: placing the diaphragm into an atomic layer deposition device and performing cyclic deposition to obtain a composite diaphragm with a conductive ion layer deposited on the outer surface of the diaphragm layer;
[0036] S2: subjecting the composite separator to cyclic deposition to obtain a modified battery separator having a modified layer deposited on the outer surface of the separator layer.
[0037] According to some preferred embodiments of the present invention, in step S1, the depositing step includes:
[0038] S1.1: placing the diaphragm in a chamber of an atomic deposition device, lowering the gas pressure to below 0.05 to 1 Torr, and then introducing a small amount of inert gas to maintain the fluidity of the inert gas in the chamber;
[0039] S1.2: introducing reactant oxidizing gas into the chamber to maintain pressure for reaction;
[0040] S1.3: Pulsing the precursor of the conductive ion layer into the chamber to complete one pulse, flushing with an inert gas for the first time, and then pulsing the reactant into the chamber to complete the second flushing with an inert gas to obtain a composite membrane;
[0041] According to some embodiments of the present invention, in step S1.2, the inert gas includes at least one of nitrogen and argon.
[0042] According to some embodiments of the present invention, in step S1.2, the amount of the oxidizing gas introduced is 100 to 50,000 sccm.
[0043] According to some embodiments of the present invention, in step S1.2, the oxidizing gas includes at least one of oxygen plasma, ozone and water vapor.
[0044] According to some embodiments of the present invention, in step S1.2, the pressure-maintaining reaction is carried out at a pressure of 0.01-50 Torr for 0.1-500 s.
[0045] According to some embodiments of the present invention, in step S1.3, the inert gas includes at least one of nitrogen and argon.
[0046] According to some embodiments of the present invention, in step S1.3, the precursor pulse of the conductive ion layer enters the chamber to complete the reaction conditions of one pulse: the air pressure in the chamber is 0.01-50 Torr, the valve switching time is 0.1-50s, the pressure holding time is 0.1-100s, and the number of times is 1-1000 times.
[0047] According to some embodiments of the present invention, in step S1.3, the precursor of the conductive ion layer includes at least one of a metal organic compound and a metal inorganic compound.
[0048] According to some embodiments of the present invention, the metal organic compound is MR n , M is the metal atom, R is the organic group, and n is the coordination number.
[0049] According to some embodiments of the present invention, the metal inorganic compound comprises a metal chloride.
[0050] According to some embodiments of the present invention, the precursor of the conductive ion layer includes at least one of diethylzinc, bis(2,2,6,6,-tetramethyl-3,5-heptanedione)zinc, tetrakis(dimethylamino)zirconium and tetrakis(ethylamino)zirconium.
[0051] According to some embodiments of the present invention, in step S1.3, the time of the first purge of the inert gas is 1-500 s.
[0052] According to some embodiments of the present invention, in step S1.3, the reactant includes at least one of an oxidizing gas such as water, hydrogen peroxide, oxygen, ozone, and plasma oxygen.
[0053] According to some embodiments of the present invention, in step S1.3, the reaction conditions for pulsing the reactant into the cavity are:
[0054] The valve opening and closing time is 0.1 to 50 seconds, the pressure holding time is 1 to 500 seconds, and the number of times is 1 to 50 times.
[0055] According to some embodiments of the present invention, in step S1.3, the second purge time of the inert gas is 1-1000 s.
[0056] According to some embodiments of the present invention, step S1.3 is a one-cycle deposition, and the composite membrane is obtained after the number of cycle deposition is 5 to 1000 times.
[0057] According to some embodiments of the present invention, in step S1, the temperature of the cyclic deposition is 20-300°C.
[0058] According to some embodiments of the present invention, in step S2, the temperature of the cyclic deposition is 20-300°C.
[0059] According to some preferred embodiments of the present invention, in step S2, the depositing step includes:
[0060] S2.1: Pulse the precursor of the modification layer into the chamber to complete one pulse, purge with inert gas for the third time, pulse the reactant into the chamber to complete the fourth purge with inert gas to obtain a modified battery separator.
[0061] According to some embodiments of the present invention, in step S2.1, the reaction conditions for the precursor pulse of the modification layer to enter the chamber to complete one pulse are: valve switching time is 0.1 to 100 s, pressure holding time is 0.1 to 100 s, and the number of times is 1 to 5 times.
[0062] According to some embodiments of the present invention, in step S2.1, the precursor of the modified layer includes a metal organic compound, and the metal compound is MR n, M is a metal atom, R is an organic group, n is the coordination number, and it can also be a metal inorganic compound, such as a metal chloride.
[0063] According to some embodiments of the present invention, in step S2.1, the time for the third purge of the inert gas is 1 to 100 seconds.
[0064] According to some embodiments of the present invention, in step S2.1, the reactant includes at least one of an oxidizing gas such as water, hydrogen peroxide, oxygen, ozone, and plasma oxygen.
[0065] According to some embodiments of the present invention, in step S2.1, the reaction conditions for pulsing the reactants into the cavity are: valve switching time is 0.1 to 5 s, pressure holding time is 1 to 100 s, and the number of times is 1 to 10 times.
[0066] According to some embodiments of the present invention, in step S2.1, the fourth purge of the inert gas lasts for 1 to 180 seconds.
[0067] According to some embodiments of the present invention, step S2.1 is a one-time cyclic deposition, and the outer surface modification layer of the composite diaphragm is obtained after the cyclic deposition number is 1 to 500 times.
[0068] According to some preferred embodiments of the present invention, the method for preparing the modified battery separator comprises:
[0069] A1: placing the diaphragm into an atomic layer deposition device and performing cyclic deposition to obtain a composite diaphragm with a conductive ion layer deposited on the outer surface of the diaphragm layer;
[0070] A2: The composite separator is subjected to cyclic deposition to obtain a modified battery separator having a modified layer deposited on the outer surface of the separator layer.
[0071] A3: The conductive ion layer and the modified layer are cyclically stacked on the outer surface of the modified battery separator, and the number of cycles is 1 to multiple times, for example, 1 time, 2 times or 3 times.
[0072] According to some preferred embodiments of the present invention, in step S1, the depositing step includes:
[0073] A1.1: Place the diaphragm in the chamber of the atomic deposition equipment, lower the gas pressure to below 0.05-1 Torr, and then introduce a small amount of inert gas to maintain the fluidity of the inert gas in the chamber;
[0074] A1.2: Introduce oxidizing gas into the chamber to maintain pressure reaction;
[0075] A1.3: Pulse the precursor of the conductive ion layer into the chamber to complete one pulse, purge it with inert gas for the first time, pulse the reactant into the chamber to complete the second purge with inert gas to obtain the composite membrane;
[0076] According to some embodiments of the present invention, in step A1.2, the amount of the oxidizing gas introduced is 100-1000 sccm.
[0077] According to some embodiments of the present invention, in step A1.2, the pressure-maintaining reaction is carried out at 1-50 Torr for 5-500 s.
[0078] According to some embodiments of the present invention, in step A1.3, the precursor pulse of the conductive ion layer enters the chamber to complete the reaction conditions of one pulse: valve switching time is 0.1 to 5 s, pressure holding time is 1 to 20 s, and the number of times is 1 to 5 times.
[0079] According to some embodiments of the present invention, in step A1.3, the precursor of the conductive ion layer includes at least one of a metal organic compound and a metal inorganic compound.
[0080] According to some embodiments of the present invention, the metal organic compound is MR n , M is the metal atom, R is the organic group, and n is the coordination number.
[0081] According to some embodiments of the present invention, the metal inorganic compound comprises a metal chloride.
[0082] According to some embodiments of the present invention, the precursor of the conductive ion layer includes at least one of diethylzinc, bis(2,2,6,6,-tetramethyl-3,5-heptanedione)zinc, tetrakis(dimethylamino)zirconium and tetrakis(ethylamino)zirconium.
[0083] According to some embodiments of the present invention, in step A1.3, the first purge of the inert gas lasts for 30-150 seconds.
[0084] According to some embodiments of the present invention, in step A1.3, the reactant includes at least one of an oxidizing gas such as water, hydrogen peroxide, oxygen, ozone, and plasma oxygen.
[0085] According to some embodiments of the present invention, in step A1.3, the reaction conditions for pulsing the reactant into the cavity are:
[0086] The valve opening and closing time is 0.1 to 5 seconds, the pressure holding time is 1 to 20 seconds, and the number of times is 1 to 5 times.
[0087] According to some embodiments of the present invention, in step A1.3, the second purge time of the inert gas is 30 to 360 seconds.
[0088] According to some embodiments of the present invention, the step A1.3 is a one-time cyclic deposition, and the number of cyclic depositions is 3 to 20 times.
[0089] According to some preferred embodiments of the present invention, in step A2, the depositing step includes:
[0090] A2.1: Pulse the precursor of the modification layer into the chamber once, purge it with inert gas for the third time, pulse the reactant into the chamber once, and purge it with inert gas for the fourth time.
[0091] According to some embodiments of the present invention, in step A2.1, the reaction conditions for the precursor pulse of the modification layer to enter the chamber to complete one pulse are: valve switching time is 0.1 to 5 s, pressure holding time is 1 to 20 s, and the number of times is 1 to 5 times.
[0092] According to some embodiments of the present invention, in step A2.1, the precursor of the conductive ion layer includes at least one of a metal organic compound and a metal inorganic compound.
[0093] According to some embodiments of the present invention, the metal organic compound is MR n , M is the metal atom, R is the organic group, and n is the coordination number.
[0094] According to some embodiments of the present invention, the metal inorganic compound comprises a metal chloride.
[0095] According to some embodiments of the present invention, the precursor of the conductive ion layer includes at least one of diethylzinc, bis(2,2,6,6,-tetramethyl-3,5-heptanedione)zinc, tetrakis(dimethylamino)zirconium and tetrakis(ethylamino)zirconium.
[0096] According to some embodiments of the present invention, in step A2.1, the third purge of the inert gas lasts for 30 to 90 seconds.
[0097] According to some embodiments of the present invention, in step A2.1, the reactant includes at least one of water, hydrogen peroxide, oxygen, ozone, etc. and plasma oxygen.
[0098] According to some embodiments of the present invention, in step A2.1, the reaction conditions for pulsing the reactant into the chamber are:
[0099] The valve opening and closing time is 0.1 to 5 seconds, the pressure holding time is 1 to 20 seconds, and the number of times is 1 to 5 times.
[0100] According to some embodiments of the present invention, in step A2.1, the fourth purge time of the inert gas is 30 to 180 seconds.
[0101] According to some embodiments of the present invention, the step A2.1 is a one-time cyclic deposition, and the modified layer of the composite membrane is obtained after the cyclic deposition number is 2-40 times.
[0102] According to some embodiments of the present invention, step A3 includes repeating steps A1.3 to A2.1 2 to 5 times to obtain a PE diaphragm modified with an ion-conducting layer / modification layer nano-laminated structure.
[0103] In some embodiments of the present invention, the method for preparing the modified battery separator further comprises a spatial atomic layer deposition preparation method.
[0104] The spatial atomic deposition preparation method is to place a diaphragm in the atomic layer deposition system chamber, and after evacuation, introduce the isolation gas, precursor, and oxygen-containing reactant into the atomic layer deposition chamber in sequence or simultaneously; start the moving mechanism to move the diaphragm through the deposition area of the chamber one or more times to obtain the ion-conducting layer and the modification layer.
[0105] According to some embodiments of the present invention, the precursor includes at least one of diethylzinc, bis(2,2,6,6,-tetramethyl-3,5-heptanedione)zinc, tetrakis(dimethylamino)zirconium and tetrakis(ethylamino)zirconium.
[0106] According to some embodiments of the present invention, the reactant comprises at least one of H2O, oxygen and ozone.
[0107] According to some embodiments of the present invention, the moving mechanism has a moving speed of 0.1 m-300 / min.
[0108] According to an embodiment of the third aspect of the present invention, application of the modified battery separator in an ion battery is proposed.
[0109] According to some embodiments of the present invention, the ion battery includes one of a sodium ion battery, a zinc ion battery and a lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] Figure 1 The ion migration number test result of the modified battery separator of Example 1;
[0111] Figure 2 Ion migration number test results of the untreated PE diaphragm of Comparative Example 1;
[0112] Figure 3 This is a thermal shrinkage performance test of the modified battery separator of Example 2 and a thermal shrinkage performance test of the untreated PE separator of Comparative Example 1.
[0113] Figure 4 Wettability test of the modified diaphragm of Example 3 to polar solutions;
[0114] Figure 5 This is a wettability test of the untreated PE diaphragm of Comparative Example 1 to polar solutions. Specific embodiments
[0115] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0116] Embodiment 1:
[0117] This embodiment prepares a modified battery separator, and the specific steps are as follows:
[0118] B1: Place the PE membrane in the chamber of the atomic layer deposition system. After evacuation, introduce the inert gas N2 / Ar, zinc precursor diethylzinc or bis(2,2,6,6,-tetramethyl-3,5-heptanedione)zinc, and reactant H2O / oxygen / ozone (O2 / O3) mixed gas into the space-type atomic layer deposition system simultaneously or step by step. The introduction rate of N2 / Ar is 0.1-100SLM.
[0119] B2: Start the moving mechanism with a moving speed of 0.1m-300 / min, so that the diaphragm moves through the deposition area of the system at least once to form a composite membrane of the ion-conducting layer and the modification layer, and a modified battery diaphragm with 5nm ZnO / 5nm ZrO2 film deposited on the inner pores and outer surface of the PE diaphragm.
[0120] Figure 1 The ion migration number test results of the modified battery separator in Example 1 are shown in FIG.
[0121] Embodiment 2:
[0122] This embodiment prepares a modified battery separator. The difference between this embodiment and embodiment 1 is that the conductive ion layer is Li5La3Nb2O 12 , the modified layer is AlN, and the other conditions are the same as those in Example 1. Figure 3 This is a thermal shrinkage performance test of the modified battery separator of Example 2.
[0123] Example 3
[0124] This example prepares a modified battery separator. The difference between this example and Example 1 is that the conductive ion layer is Li x La y Ti z O, x+3y+4z=2, the modified layer is CeF3, and the other conditions are the same.
[0125] Example 4
[0126] In this embodiment, a modified battery separator is prepared. The difference between this embodiment and embodiment 1 is that the conductive ion layer is LiPON, the modified layer is Nb2O5, and the other conditions are the same.
[0127] Example 5
[0128] In this embodiment, a modified battery separator is prepared. The difference between this embodiment and embodiment 1 is that the conductive ion layer is Y2O3, the modified layer is BN, and the other conditions are the same.
[0129] Example 6
[0130] In this embodiment, a modified battery separator is prepared. The difference between this embodiment and embodiment 1 is that the conductive ion layer is Cr2O3, the modification layer is SmF3, and the other conditions are the same.
[0131] Example 7
[0132] This embodiment provides a modified battery separator, and the preparation method is as follows:
[0133] B3: Depositing HfO2 film on the inner pores and outer surface of PE diaphragm using atomic layer deposition;
[0134] B3.1: At 60-150°C, pulse the hafnium source into the reaction chamber, valve switch time: 0.01-5s, ALD reaction chamber pressure reaches 0.05-5Torr, precursor pressure holding time 1-50s, number of times 1-5 times;
[0135] B3.2: 1000-20000sccm N2 purge time 10-500s;
[0136] B3.3: The reactant H2O is pulsed into the reaction chamber, the valve switch time is 0.01-5s, the ALD reaction chamber pressure reaches 0.05-5Torr, the H2O pressure holding time is 1-50s, and the number of times is 1-5 times;
[0137] B3.4: 1000-20000sccm N2 purge time 10-500s;
[0138] The four steps B3.1 to B3.4 are cycled for 5 to 50 times to obtain a composite membrane with HfO2 film deposited on the inner pores and outer surface of the PE membrane;
[0139] B4.1: At 30-150°C, pulse the precursor trimethylaluminum into the reaction chamber, valve switch time: 0.1-5s, ALD reaction chamber pressure reaches 0.05-5Torr, precursor pressure holding time 0.1-50s, number of times 1;
[0140] B4.2: 1000-20000sccm N2 purge time 10-500s;
[0141] B4.3: The reactant NH3 is pulsed into the reaction chamber, the valve switch time is 0.1-5s, the ALD reaction chamber pressure reaches 0.05-5Torr, the NH3 pressure holding time is 0.1-5s, and the number of times is 1-5 times;
[0142] B4.4: 1000-20000sccm N2 purge time 10-500s;
[0143] The four steps B4.1 to B4.4 are cycled 5-50 times to obtain a modified battery separator.
[0144] Example 8
[0145] This embodiment provides a modified battery separator. The difference between this embodiment and embodiment 1 is that the modified battery separator has a ZnO / ZrO2 / ZnO / ZrO2 film deposited on the inner pores and outer surface of the PE separator, and the other conditions are the same.
[0146] Comparative Example 1
[0147] This comparative example provides an unmodified PE membrane. The ion migration number test results of the untreated PE membrane of comparative example 1 are as follows: Figure 2 shown.
[0148] Comparative Example 2
[0149] In this example, a modified battery separator is prepared. The difference between this comparative example and Example 1 is that the conductive ion layer is ZnO and there is no modification layer, and the other conditions are the same.
[0150] Comparative Example 3
[0151] In this embodiment, a modified battery separator is prepared. The difference between this embodiment and embodiment 1 is that the conductive ion layer is Li3PO4 and there is no modification layer. The other conditions are the same.
[0152] Test Example 1
[0153] This test example tests the ion migration number of the membranes of Comparative Example 1 and Example 1. Figure 1 As shown in Figure 2, the ion migration number of the untreated PE diaphragm (Comparative Example 1) is 0.19, while the ion migration number of the diaphragm coated with ZnO / ZrO2 on the surface (Example 1) is increased to 0.53, which is more than doubled. This shows that the ion conductivity of the diaphragm surface has been effectively improved.
[0154] Test Example 2
[0155] This test example tests the surface shrinkage of Example 2 and Comparative Example 1 after being kept at 150°C for 1 hour. The surface shrinkage of the modified battery separator of Example 2 is only 24% (as shown in Figure 2). Figure 3 A), B), while the untreated PE diaphragm surface shrinkage of Comparative Example 1 is 88%, much greater than 30% (as shown in Figure 3 (as shown in C) and D) in the figure).
[0156] Test Example 3
[0157] Test Example 3 tested the untreated comparative example 1 diaphragm and example 3 PE-Li x La y Ti z The size of the O / CeF3 electrolyte contact angle, such as Figure 4 As shown in Figure 5, the contact angle of the PE surface after ALD coating is reduced from the original 67.7° to 19.6°, and the wettability of the electrolyte is significantly improved.
[0158] Test Example 4
[0159] Preparation and testing of lithium-ion batteries in the embodiments and comparative examples:
[0160] The positive electrode LiNi 0.8 Co 0.1 Mn 0.1 O2 NCM811 and graphite negative electrode were assembled into a soft pack battery with a capacity of 1Ah, and the charge and discharge cycle test was carried out at room temperature under the condition of 1C / 1C. The original PE separator was used as comparative example 1, and the comparison of the number of cycles with the ALD-PE comparative example and the embodiment is listed in Table (1).
[0161] At the same time, the withstand voltage results of the diaphragm are also compared in Table (1). The withstand voltage test is conducted in accordance with the national standard GB / T1408.1-2016.
[0162] Table 1 Battery performance comparison
[0163]
[0164]
[0165] As can be seen from Table 1, the number of cycles of the single-layer modified layer at 80% capacity retention rate has increased by about 54% compared to the control sample. At the same time, the double-layer modified layer can further improve the cycle performance, and the increase in the number of cycles is more than 90%. This shows that the double-layer modified layer can better improve the cycle performance of the diaphragm. At the same time, the double-layer modified layer can improve the voltage resistance performance of the diaphragm by more than 55%.
[0166] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A modified battery separator, characterized in that: The battery separator is: a diaphragm; a hole in the diaphragm; Conductive ion layer; the conductive ion layer is arranged on the outer surface of the diaphragm layer; A modified layer; the modified layer is disposed on the outer surface of the conductive ion layer; The raw material for preparing the conductive ion layer is Li5La3Nb2O 12 ; The raw material for preparing the modified layer is AlN; The conductive ion layer and the modified layer are sequentially disposed on the diaphragm by atomic layer deposition; The thickness of the conductive ion layer is 0.1-20 nm; The thickness of the modified layer is 0.1-20 nm.
2. The modified battery separator according to claim 1, characterized in that: The separator includes at least one of a polyethylene separator, a polypropylene separator, a polyethylene and polypropylene multilayer separator, a Celgard separator, and a polyimide separator.
3. A method for preparing a modified battery separator as claimed in claim 1 or 2, characterized in that: include: The diaphragm is placed in the chamber of the atomic layer deposition system, and after evacuation, the isolation gas, the precursor, and the oxygen-containing reactant are introduced into the atomic layer deposition chamber in sequence or simultaneously; The moving mechanism is started to move the membrane through the deposition area of the cavity one or more times, thereby obtaining the conductive ion layer and the modified layer.
4. Use of the modified battery separator according to claim 1 or 2 in ion batteries.
Citation Information
Patent Citations
Preparation method of modified PP / PE / PP diaphragm and application of diaphragm
CN114883744A