A kind of high wear-resistant UV sag ink and preparation method thereof

By using nano-alumina modified PUA resin and high-function wear-resistant resin in inkjet printing ink, the problem of lack of wear resistance of decorative patterns is solved, and the high wear resistance of ink coating is achieved and the production process is simplified, avoiding the Use of additional wear-resistant layers.

CN116751482BActive Publication Date: 2024-11-22GUANGDONG HEYGEY LIGHT CURING MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310454519.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-22
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

The decorative patterns formed by inkjet printing technology on the floor surface lack wear resistance. The existing solutions require the installation of PVC wear-resistant layers on the pattern surface, which is complicated in process, low in efficiency and high cost.

Method used

Using nano-alumina modified PUA resin and high-function wear-resistant resin and other materials, high-wear-resistant UV sinking ink is synthesized through specific preparation methods. The ink coating itself has good wear resistance, avoiding the installation of wear-resistant layers on the surface. need.

Benefits of technology

The production process is simplified, efficiency is improved, and the wear resistance and transparency of the ink coating are enhanced without affecting gloss.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of ink technology, and in particular to a highly wear-resistant UV sinking ink and a preparation method thereof. Inkjet printing technology can be used to form exquisite decorative patterns on the surface of a floor, but the formed decorative patterns usually do not have good wear resistance. The present invention provides a highly wear-resistant UV sinking ink, wherein a nano-alumina-modified PUA resin is added to the highly wear-resistant UV sinking ink system, wherein the nano-alumina-modified PUA resin is a polyurethane resin structure in which nano-alumina inorganic nanoparticles are introduced. On the one hand, the problem that nano-alumina is easy to agglomerate and difficult to disperse in the ink system is overcome, and on the other hand, the problem that nano-alumina is poorly compatible with the ink system is overcome, which plays a beneficial role in improving the wear resistance and other properties of the ink system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, and in particular to a highly wear-resistant UV sag ink and a preparation method thereof. Background Art

[0002] At present, inkjet printing technology can be used to form exquisite decorative patterns on the floor surface, but the formed decorative patterns usually do not have good wear resistance. In order to solve this problem, a PVC wear-resistant layer is usually set on the surface of the decorative pattern, and the PVC wear-resistant layer is bonded to the decorative pattern by an adhesive. Although this method can give the floor better wear resistance, the process is relatively complicated, the efficiency is low, and the production cost is high.

[0003] Based on the above problems, the present invention provides a highly wear-resistant UV sag ink, whose material system is added with the homemade nano-alumina modified PUA resin of the present invention and other wear-resistant additives. The cured ink coating itself has good wear resistance, and there is no need to set a wear-resistant layer on the surface of the ink coating, which simplifies the production process and improves efficiency. Summary of the invention

[0004] The technical problem to be solved by the present invention is that a beautiful decorative pattern can be formed on the floor surface by inkjet printing technology, but the formed decorative pattern usually does not have good wear resistance. The present invention provides a highly wear-resistant UV sinking ink, which comprises the following components in parts by weight:

[0005] Nano-alumina modified PUA resin 10-20 parts

[0006] 10-20 parts of high-functional wear-resistant resin

[0007] Active monomer 30-50 parts

[0008] Wear-resistant filler 20-30 parts

[0009] 3-5 parts of photoinitiator

[0010] 1-5 parts of additives

[0011] Anti-settling agent 0.2-1 part.

[0012] Specifically, the preparation method of the nano-alumina modified PUA resin, in parts by weight, comprises the following steps:

[0013] (1) Add 20 parts of nano-alumina and 60 parts of butyl acetate to a reaction kettle with a reflux device, and disperse them by ultrasonic at 60°C for 1 hour. Then, drop 20 parts of KH570 into the system and complete the dropwise addition within 30 minutes. Then, place the reaction system at 60°C and stir at high speed for 1 hour to obtain a modified alumina sol.

[0014] (2) Add 20 parts of pentaerythritol triacrylate and 60 parts of 6-functionality aliphatic polyurethane acrylate into a reaction kettle, stir and mix evenly, then stir and heat to 60°C, then add 20 parts of the modified alumina sol obtained in step (1) into the reaction system, and then stir and react at 60°C for 2 hours to obtain nano-alumina modified PUA resin.

[0015] Specifically, the high-functional wear-resistant resin includes at least one of aliphatic polyurethane acrylic resins with functionality of 9-18.

[0016] Specifically, the 9-18 functionality aliphatic polyurethane acrylic resin includes at least one of aliphatic polyurethane acrylic resins L-6901, L-6902, 6195-100 or ST8915.

[0017] Specifically, the reactive monomer includes at least one of tripropylene glycol diacrylate, dipropylene glycol diacrylate, hexanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.

[0018] Specifically, the wear-resistant filler includes at least one of ultrafine high-hardness ceramic powder, glass powder, alumina, polyethylene wax, polytetrafluoroethylene wax, and acrylic microspheres.

[0019] Specifically, the photoinitiator includes at least one of 1-hydroxycyclohexyl phenyl ketone, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, methyl benzoylformate, and bis (2,6-difluoro-3-pyrrolophenyl) titanocene.

[0020] Specifically, the auxiliary agent includes at least one of a dispersant, a leveling agent, and an adhesion promoter.

[0021] Specifically, the anti-settling agent includes at least one of fumed silica and bentonite.

[0022] Specifically, the preparation method of the highly wear-resistant UV sag ink comprises the following steps:

[0023] In an environment where a yellow light is used and ultraviolet light is completely blocked, the active monomer, photoinitiator and additive are mixed and stirred at 300 rpm until dissolved. After dissolution, nano-alumina-modified PUA resin and high-functional wear-resistant resin are added in sequence and stirred at 800 rpm to mix evenly. Then, wear-resistant filler and anti-settling agent are added in sequence and dispersed at a high speed of 1500 rpm for 30 minutes to obtain a highly wear-resistant UV sinking ink.

[0024] The beneficial effects of the present invention are:

[0025] (1) The high wear-resistant UV sag ink system of the present invention contains nano-alumina modified PUA resin, which is a polyurethane resin structure in which nano-alumina inorganic nanoparticles are introduced. On the one hand, the problem that nano-alumina is easy to agglomerate and difficult to disperse in the ink system is overcome; on the other hand, the problem that nano-alumina is poorly compatible with the ink system is overcome, which plays a beneficial role in improving the wear resistance and other properties of the ink system.

[0026] (2) The 6-functionality polyurethane acrylate used in the modification process of the nano-alumina modified PUA resin of the present invention is aliphatic, which has better compatibility with the high-functionality wear-resistant resin (aliphatic) in the ink system, and also plays a role that cannot be ignored in further improving the wear resistance of the ink system;

[0027] (3) The present invention introduces nano-alumina into the ink system in this way, so that the nano-alumina is grafted into the resin system, so that the cured ink coating has higher transparency and has no effect on the glossiness of the cured ink coating. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0029] The nano-alumina modified PUA resins in the following embodiments of the present invention are prepared according to the following steps:

[0030] (1) 20 parts of nano-alumina and 60 parts of butyl acetate were added to a reaction kettle with a reflux device, and ultrasonic dispersion was performed at 60°C for 1 hour. Then, 20 parts of KH570 were dripped into the system and the dripping was completed within 30 minutes. Then, the reaction system was placed at 60°C and stirred at high speed for 1 hour to obtain a modified alumina sol. The nano-alumina was purchased from Beijing Dekedaojin Technology Co., Ltd. with a grade of DK410-1 and an average particle size of 20 nm.

[0031] (2) Add 20 parts of pentaerythritol triacrylate and 60 parts of 6-functionality aliphatic polyurethane acrylate into a reaction kettle, stir and mix evenly, then stir and heat to 60°C, then add 20 parts of the modified alumina sol obtained in step (1) into the reaction system, then stir and react at 60°C for 2h to obtain nano-alumina modified PUA resin, wherein the 6-functionality aliphatic polyurethane acrylate is ETERCURE6150-100 from Taiwan, China.

[0032] The additives in the following embodiments of the present invention are composed of a dispersant, a leveling agent, and an adhesion promoter in a mass ratio of 1:1:1. The dispersant is EKKA4310, the leveling agent is BYK-306, and the adhesion promoter is Sartomer CD9051.

[0033] The ultrafine high hardness ceramic powder in the following embodiments of the present invention is of model SAR-10, purchased from Hangzhou Weiwei Nano Technology Co., Ltd.

[0034] The fumed silica in the following embodiments of the present invention is Evonik Degussa A380.

[0035] The average particle size of the glass powder in the following examples of the present invention is 1200 mesh, which is purchased from Shijiazhuang Hangquan Mineral Products Co., Ltd.

[0036] The bentonite in the following examples of the present invention is BENGEL 828 from Hemmingsdeqian.

[0037] The wear-resistant filler alumina grade in the following embodiments of the present invention is CLS-8, purchased from Shijiazhuang Hangquan Mineral Products Co., Ltd.

[0038] The polyethylene wax in the following examples of the present invention is PEW-0221, purchased from Nanjing Tianshi New Material Technology Co., Ltd.

[0039] The polytetrafluoroethylene wax in the following embodiments of the present invention is PTEF-0103, purchased from Nanjing Tianshi New Material Technology Co., Ltd.

[0040] The acrylic microspheres in the following embodiments of the present invention are of brand DA-980, purchased from Guangzhou Sandinghui Trading Co., Ltd.

[0041] Example 1

[0042] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0043] Nano-alumina modified PUA resin 10 parts

[0044] Aliphatic polyurethane acrylic resin L-6901 10 parts

[0045] 30 parts of tripropylene glycol diacrylate

[0046] 20 parts of ultra-fine high hardness ceramic powder

[0047] 3 parts of photoinitiator

[0048] 1 part of additive

[0049] 0.2 parts of fumed silica.

[0050] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0051] Example 2

[0052] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0053] 20 parts of nano-alumina modified PUA resin

[0054] Aliphatic polyurethane acrylic resin L-6902 20 parts

[0055] 50 parts of propylene glycol diacrylate

[0056] 30 parts glass powder

[0057] Photoinitiator 5 parts

[0058] 5 parts of additives

[0059] 1 part bentonite.

[0060] The photoinitiator is composed of methyl benzoylformate and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0061] Example 3

[0062] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0063] Nano-alumina modified PUA resin 12 parts

[0064] Aliphatic polyurethane acrylic resin 6195-100 10 parts

[0065] 31 parts of hexanediol diacrylate

[0066] 22 parts of aluminum oxide

[0067] 3 parts of photoinitiator

[0068] 1 part of additive

[0069] 0.2 parts of fumed silica.

[0070] The photoinitiator is composed of bis-2,6-difluoro-3-pyrrolephenyl titanocene and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0071] Example 4

[0072] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0073] Nano-alumina modified PUA resin 13 parts

[0074] Aliphatic polyurethane acrylic resin ST8915 12 parts

[0075] 35 parts of trimethylolpropane triacrylate

[0076] 24 parts of polyethylene wax

[0077] 3 parts of photoinitiator

[0078] 2 parts of additives

[0079] 0.2 parts of bentonite.

[0080] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0081] Example 5

[0082] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0083] Nano-alumina modified PUA resin 15 parts

[0084] Aliphatic polyurethane acrylic resin L-6901 13 parts

[0085] Pentaerythritol triacrylate 32 parts

[0086] 25 parts of polytetrafluoroethylene wax

[0087] 3 parts of photoinitiator

[0088] 2 parts of additives

[0089] 0.4 parts of bentonite.

[0090] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0091] Example 6

[0092] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0093] Nano-alumina modified PUA resin 17 parts

[0094] Aliphatic polyurethane acrylic resin L-6902 15 parts

[0095] Pentaerythritol tetraacrylate 38 parts

[0096] Acrylic microspheres 25 pieces

[0097] Photoinitiator 4 parts

[0098] 3 parts of additives

[0099] 0.5 parts of fumed silica.

[0100] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0101] Example 7

[0102] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0103] Nano-alumina modified PUA resin 18 parts

[0104] Aliphatic polyurethane acrylic resin ST8915 16 parts

[0105] 42 parts of dipentaerythritol hexaacrylate

[0106] 27 parts of ultra-fine high hardness ceramic powder

[0107] Photoinitiator 4 parts

[0108] 4 parts of additives

[0109] 1 part of fumed silica.

[0110] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0111] Example 8

[0112] A highly wear-resistant UV sag ink, in parts by weight, is composed as follows:

[0113] 20 parts of nano-alumina modified PUA resin

[0114] Aliphatic polyurethane acrylic resin 6195-100 18 parts

[0115] 46 parts of pentaerythritol tetraacrylate

[0116] Acrylic microspheres 27 pieces

[0117] Photoinitiator 5 parts

[0118] 5 parts of additives

[0119] 1 part bentonite.

[0120] The photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide in a mass ratio of 2:1.

[0121] Comparative Example 1 is the same as Example 1, except that, in Comparative Example 1, a mixture of modified alumina sol and 6-functionality aliphatic polyurethane acrylate (ETERCURE 6150-100, Changxing, Taiwan, China) in equal parts by weight is used to replace the nano-alumina modified PUA resin in Example 1, and the weight ratio of the modified alumina sol to ETERCURE 6150-100, Changxing, Taiwan, China is 1:3. The preparation method of the modified alumina sol is as follows:

[0122] 20 parts of nano-alumina and 60 parts of butyl acetate were added to a reactor with a reflux device, and ultrasonic dispersion was carried out at 60°C for 1 hour. Then, 20 parts of KH570 were dripped into the system and the addition was completed within 30 minutes. Then, the reaction system was placed at 60°C and stirred at high speed for 1 hour to obtain a modified alumina sol. The nano-alumina was of grade DK410-1 and had an average particle size of 20 nm, which was purchased from Beijing Dekedaojin Technology Co., Ltd.

[0123] Comparative Example 2 is the same as Example 1, except that, in the process of preparing nano-alumina-modified PUA resin, an equal weight portion of 6-functionality aromatic polyurethane acrylate is used to replace the 6-functionality aliphatic polyurethane acrylate in Example 1, and the model of the 6-functionality aromatic polyurethane acrylate is 305, which is purchased from Jining Juyue New Materials Co., Ltd.

[0124] Comparative Example 3 is the same as Example 1. In the process of preparing the nano-alumina-modified PUA resin in Comparative Example 3, 30 parts of the modified alumina sol obtained in step (1) are added in step (2).

[0125] Performance Testing

[0126] The inks obtained in Examples 1-8 and Comparative Examples 1-3 of the present invention were sprayed on the surface of the PVC film material, and the photocuring thickness was 30 μm. Then, the ink curing coatings obtained in Examples 1-8 and Comparative Examples 1-3 were respectively tested for relevant properties. The test results are shown in Table 1.

[0127] Adhesion: Tested according to the cross-cut test for paint and varnish films in GB9286-88.

[0128] Hardness: Tested in accordance with GB / T6739-2006.

[0129] Wear resistance: Use Taber5155 abrasion tester, CS-10 abrasion wheel, load 1000G, and test at a speed of 72 rpm. Observe until the paint film is worn through and the substrate is exposed, and record the current number of turns.

[0130] Table 1

[0131] Test items Adhesion hardness Wear resistance (circle) Example 1 5B 3H 700 Example 2 4B 5H 1500 Example 3 5B 3H 800 Example 4 5B 3H 700 Example 5 5B 3H 800 Example 6 5B 4H 900 Example 7 4B 4H 1300 Example 8 4B 5H 1200 Comparative Example 1 4B 2H 500 Comparative Example 2 4B 3H 600 Comparative Example 3 4B 2H 500

[0132] The above description is only illustrative rather than restrictive of the present invention. Those skilled in the art will understand that many modifications, changes or equivalents may be made without departing from the spirit and scope defined by the appended claims, but all will fall within the scope of protection of the present invention.

Claims

1. A highly wear-resistant UV sag ink, characterized in that: In parts by weight, it is composed of the following ingredients: Nano-alumina modified PUA resin 10-20 parts 10-20 parts of high-functional wear-resistant resin Active monomer 30-50 parts 20-30 parts of wear-resistant filler 3-5 parts of photoinitiator 1-5 parts of additives Anti-settling agent 0.2-1 part; The preparation method of the nano-alumina modified PUA resin, in parts by weight, comprises the following steps: (1) Add 20 parts of nano-alumina and 60 parts of butyl acetate to a reaction kettle with a reflux device, and disperse them by ultrasonic at 60° C. for 1 hour. Then, add 20 parts of KH570 dropwise into the system and complete the addition within 30 minutes. Then, place the reaction system at 60° C. and stir at high speed for 1 hour to obtain a modified alumina sol; (2) Add 20 parts of pentaerythritol triacrylate and 60 parts of 6-functionality aliphatic polyurethane acrylate into a reaction kettle, stir and mix evenly, then stir and heat to 60° C., then add 20 parts of the modified alumina sol obtained in step (1) into the reaction system, and then stir and react at 60° C. for 2 hours to obtain nano-alumina modified PUA resin; The high-functional wear-resistant resin includes at least one of 9-18 functional aliphatic polyurethane acrylic resins; The 9-18 functionality aliphatic polyurethane acrylic resin includes at least one of aliphatic polyurethane acrylic resins L-6901, L-6902, 6195-100 or ST8915.

2. A highly wear-resistant UV sag ink according to claim 1, characterized in that: The reactive monomer includes at least one of tripropylene glycol diacrylate, dipropylene glycol diacrylate, hexanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.

3. A highly wear-resistant UV sag ink according to claim 1, characterized in that: The wear-resistant filler includes at least one of ultra-fine high-hardness ceramic powder, glass powder, alumina, polyethylene wax, polytetrafluoroethylene wax, and acrylic microspheres.

4. The highly wear-resistant UV sag ink according to claim 1, characterized in that: The photoinitiator includes at least one of 1-hydroxycyclohexyl phenyl ketone, diphenyl (2, 4, 6-trimethylbenzoyl) phosphine oxide, methyl benzoylformate, and bis (2, 6-difluoro-3-pyrrolephenyl) titanocene.

5. The highly wear-resistant UV sag ink according to claim 1, characterized in that: The auxiliary agent includes at least one of a dispersant, a leveling agent, and an adhesion promoter.

6. The highly wear-resistant UV sag ink according to claim 1, characterized in that: The anti-settling agent includes at least one of fumed silica and bentonite.

7. A highly wear-resistant UV sag ink according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: in an environment where a yellow light is used and ultraviolet light is completely blocked, active monomers, photoinitiators and additives are mixed, stirred at 300 rpm until dissolved, nano-alumina-modified PUA resin and high-functional wear-resistant resin are added in sequence after dissolution, stirred and mixed evenly at 800 rpm, and then wear-resistant fillers and anti-settling agents are added in sequence, and dispersed at a high speed of 1500 rpm with high stirring for 30 minutes to obtain highly wear-resistant UV sinking ink.