A transition metal telluride composite carbon nanofiber, preparation method and application thereof

The preparation of transition metal telluride composite carbon nanofibers through electrospinning method solves the problems of high cost of platinum-based materials and difficult nanostructure design in electrolytic hydrogen production, and achieves high-efficiency and low-cost electrocatalytic hydrogen evolution performance, with alternative Pt The potential of /C catalyst.

CN116791237BActive Publication Date: 2024-11-22YONGHYDROGEN (CHANGZHOU) ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310746317.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-11-22
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

The catalyst with the highest catalytic activity of the cathode hydrogen evolution reaction in electrolytic water hydrogen production is a platinum-based material, but its geological reserves are limited and costly, resulting in high energy consumption and low efficiency of hydrogen production. It is difficult to design and synthesize existing transition metal chalcogen compounds with specific nanometers. Telluride of structure.

Method used

The transition metal salt and telluric acid were prepared in N,N-dimethylformamide solution by electrospinning, and doped polyacrylonitrile nanofibers were obtained by electrospinning, and formed during pre-oxidation and calcination. Transition metal telluride composite carbon nanofibers avoid the use of toxic tellurium powder.

Benefits of technology

The prepared transition metal telluride composite carbon nanofibers show excellent electrocatalytic hydrogen evolution performance in acidic and alkaline solutions, have high efficiency and low cost, and can replace commercial Pt/C catalysts, and have good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116791237B_ABST
    Figure CN116791237B_ABST
Patent Text Reader

Abstract

The invention discloses a transition metal telluride composite carbon nanofiber, a preparation method and an application thereof. The invention first uses polyacrylonitrile, a transition metal salt and telluric acid as raw materials and N,N-dimethylformamide as a solvent to prepare an electrospinning solution; then the electrospinning solution is electrospinned to obtain transition metal salt-telluric acid doped polyacrylonitrile nanofibers, and finally the nanofibers are calcined to prepare transition metal telluride composite carbon nanofibers. The transition metal telluride composite carbon nanofiber has a unique structural advantage, and is composed of transition metal telluride nanoparticles uniformly loaded on carbon nanofibers. Experimental results show that the transition metal telluride composite carbon nanofiber exhibits excellent electrocatalytic hydrogen evolution performance in both acidic and alkaline solutions, has the advantages of high hydrogen production efficiency and low economic cost, and is expected to replace commercial Pt / C catalysts, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production by electrolysis of water, and particularly relates to a transition metal telluride composite carbon nanofiber, a preparation method and application thereof. Background Art

[0002] Hydrogen production by water electrolysis is an environmentally friendly, low-carbon and sustainable large-scale hydrogen production method. However, high energy consumption and low efficiency have always been the biggest obstacles to hydrogen production by water electrolysis. Therefore, there is an urgent need to develop efficient, low-cost and stable catalysts to reduce the energy consumption of hydrogen production and improve the efficiency of hydrogen production. At present, the catalyst with the highest catalytic activity for the cathode hydrogen evolution reaction in water electrolysis is platinum-based material, but the low earth reserves and high price cost of platinum limit its large-scale commercial application.

[0003] Transition metal chalcogenides (sulfides, selenides and tellurides) have received extensive research attention as a class of efficient hydrogen evolution catalysts. Since the metallicity of tellurium is higher than that of selenium and sulfur, transition metal tellurides have higher conductivity than selenides and sulfides. Transition metal tellurides were first prepared by hydrothermal / solvothermal methods, but this method often makes it difficult to design and synthesize tellurides with specific nanostructures. Subsequently, researchers developed a method of using tellurium powder as a tellurium source, vaporizing the tellurium powder through high-temperature heat treatment and reacting it with a metal-based precursor to react with the tellurium, thereby achieving effective design of the nanostructure of transition metal tellurides. However, this method requires tellurium powder as a tellurium source, and the tail gas after the tellurium powder is vaporized easily leaks into the air, which has certain toxicity. Summary of the invention

[0004] In view of the technical problems existing in the background technology, the purpose of the present invention is to provide a transition metal telluride composite carbon nanofiber, a preparation method and its application. The transition metal telluride composite carbon nanofiber exhibits excellent electrocatalytic hydrogen evolution activity when used as a catalyst for electrolysis of water to produce hydrogen.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A first aspect of the present invention provides a method for preparing transition metal telluride composite carbon nanofibers, comprising the following steps:

[0007] S1. Preparation of electrospinning solution:

[0008] dissolving polyacrylonitrile, transition metal salt and telluric acid in N,N-dimethylformamide to prepare an electrospinning solution;

[0009] S2. Preparation of transition metal salt-telluric acid doped polyacrylonitrile nanofibers:

[0010] The electrospinning solution prepared in step S1 is transferred to an electrospinning device to obtain transition metal salt-telluric acid doped polyacrylonitrile nanofibers by electrospinning;

[0011] S3. Preparation of transition metal telluride composite carbon nanofibers:

[0012] The transition metal salt-telluric acid doped polyacrylonitrile nanofiber is placed in a tubular furnace for pre-oxidation, and then heated and calcined to obtain the transition metal telluride composite carbon nanofiber.

[0013] Preferably, in step S1, the ratio of the transition metal salt, telluric acid, N,N-dimethylformamide and polyacrylonitrile is 0.3-0.8 mmol: 0.6-1.6 mmol: 6-12 mL: 0.7-1.5 g; more preferably, it is 0.5-0.7 mmol: 1.0-1.2 mmol: 9-12 mL: 1.0-1.3 g.

[0014] Preferably, in step S2, the electrospinning conditions are: static voltage of 10-18 kV, extrusion rate of electrospinning solution of 0.1-0.5 mL / h, receiving distance of 10-30 cm, and rolling speed of receiving roller of 60-200 r / min.

[0015] Preferably, in step S3, the pre-oxidation is carried out in an air atmosphere, the pre-oxidation temperature is 250-300°C, and the pre-oxidation time is 0.5-2h; further preferably, the pre-oxidation temperature is 270-290°C, and the pre-oxidation time is 0.5-1h.

[0016] Preferably, in step S3, the calcination is carried out under an inert atmosphere, the calcination temperature is 700-1000° C., and the calcination time is 1-3 hours; more preferably, the calcination temperature is 800-900° C., and the calcination time is 1.5-2.5 hours.

[0017] The second aspect of the present invention provides transition metal telluride composite carbon nanofibers obtained by the above preparation method.

[0018] The third aspect of the present invention provides the use of the above transition metal telluride composite carbon nanofiber as a catalyst in the electrolysis of water to produce hydrogen.

[0019] The present invention has the following beneficial effects:

[0020] (1) The present invention first uses polyacrylonitrile, transition metal salt and telluric acid as raw materials and N,N-dimethylformamide as solvent to prepare an electrospinning solution; then, transition metal salt-telluric acid doped polyacrylonitrile nanofibers are obtained by electrospinning, and finally, the nanofibers are calcined to prepare transition metal telluride composite carbon nanofibers. The preparation method not only has the characteristics of simple process, controllable conditions, good repeatability, etc., but also has good universality, and can be used to prepare a series of transition metal telluride composite carbon nanofibers, while avoiding the use of toxic tellurium source-tellurium powder.

[0021] (2) The transition metal telluride composite carbon nanofiber prepared by the present invention has a unique structural advantage, and is composed of transition metal telluride nanoparticles uniformly loaded on carbon nanofibers. Among them, the carbon nanofiber not only has a high electrical conductivity, but also can improve the dispersion of transition metal telluride nanoparticles, provide more catalytic active sites, and promote electron transfer and material transport in the electrocatalytic process; experimental results show that the transition metal telluride composite carbon nanofiber prepared by the present invention exhibits excellent electrocatalytic hydrogen evolution performance in both acidic and alkaline solutions, has the advantages of high hydrogen production efficiency and low economic cost, and is expected to replace commercial Pt / C catalysts and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is the XRD pattern of the ruthenium telluride composite carbon nanofibers prepared in Example 1;

[0024] Figure 2 is the XRD pattern of the silver telluride composite carbon nanofibers prepared in Example 2;

[0025] Figure 3 is the XRD pattern of the nickel telluride composite carbon nanofibers prepared in Example 3;

[0026] Figure 4 is the XRD pattern of the copper telluride composite carbon nanofiber prepared in Example 4;

[0027] Figure 5 is a SEM image of the ruthenium telluride composite carbon nanofibers prepared in Example 1;

[0028] Figure 6 TEM image of the ruthenium telluride composite carbon nanofibers prepared in Example 1;

[0029] Figure 7 The transition metal telluride composite carbon nanofibers prepared in Examples 1-4 were heated to 0.5 MH 2 LSV curve in SO4 solution.

[0030] Figure 8 This is the LSV curve of the transition metal telluride composite carbon nanofiber prepared in Example 1-4 in 1M KOH solution. DETAILED DESCRIPTION

[0031] In the following description, for the purpose of illustration rather than limitation, specific details such as specific system structures and technologies are provided to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may also be implemented in other embodiments without these specific details.

[0032] Example 1

[0033] A method for preparing a transition metal telluride composite carbon nanofiber, specifically a ruthenium telluride composite carbon nanofiber, comprising the following steps:

[0034] S1. Preparation of electrospinning solution

[0035] Take 1 g of polyacrylonitrile, 0.5 mmol of ruthenium trichloride trihydrate and 1 mmol of telluric acid, dissolve them in 9 mL of N,N-dimethylformamide to prepare the electrospinning solution;

[0036] S2. Preparation of ruthenium trichloride-telluric acid doped polyacrylonitrile nanofibers

[0037] The electrospinning solution is loaded into the syringe of the electrospinning device. Under the action of the high voltage electric field, the electrospinning solution is stretched and extended in the air by electrospinning, and finally solidified into nanofibers on the aluminum foil of the receiving device. After the electrospinning is completed, the nanofiber membrane is placed in a drying oven for vacuum drying to obtain ruthenium trichloride-telluric acid doped polyacrylonitrile nanofibers. Among them, the static voltage is 13kV, the extrusion rate of the electrospinning solution is 0.25mL / h, the receiving distance is 20cm, and the rolling speed of the receiving roller is 90r / min.

[0038] S3. Preparation of ruthenium telluride composite carbon nanofibers:

[0039] The ruthenium trichloride-telluric acid doped polyacrylonitrile nanofibers are placed in a porcelain boat and placed in a tubular furnace. They are first pre-oxidized at 270°C for 1 hour in an air atmosphere, and then calcined at 900°C for 2 hours in an inert atmosphere. During the calcination process, ruthenium trichloride and telluric acid undergo a tellurization reaction to form ruthenium telluride, and polyacrylonitrile is carbonized into a carbon carrier material, and finally the target product, ruthenium telluride composite carbon nanofibers, is obtained.

[0040] Example 2

[0041] A method for preparing a transition metal telluride composite carbon nanofiber, specifically a silver telluride composite carbon nanofiber, comprising the following steps:

[0042] S1. Preparation of electrospinning solution

[0043] 1.3 g of polyacrylonitrile, 0.7 mmol of silver nitrate and 1.2 mmol of telluric acid were dissolved in 12 mL of N,N-dimethylformamide to prepare an electrospinning solution;

[0044] S2. Preparation of silver nitrate-telluric acid doped polyacrylonitrile nanofibers

[0045] The electrospinning solution is loaded into the syringe of the electrospinning device. Under the action of the high voltage electric field, the electrospinning solution is stretched and extended in the air by electrospinning, and finally solidified into nanofibers on the aluminum foil of the receiving device. After the electrospinning is completed, the nanofiber membrane is placed in a drying oven for vacuum drying to obtain silver nitrate-telluric acid doped polyacrylonitrile nanofibers. Among them, the static voltage is 13kV, the extrusion rate of the electrospinning solution is 0.25mL / h, the receiving distance is 20cm, and the rolling speed of the receiving roller is 90r / min.

[0046] S3. Preparation of silver telluride composite carbon nanofibers:

[0047] Silver telluride-telluric acid doped polyacrylonitrile nanofibers are placed in a porcelain boat and placed in a tubular furnace. They are first pre-oxidized at 300°C for 0.5h in an air atmosphere, and then calcined at 900°C for 2.5h in an inert atmosphere. During the calcination process, silver nitrate and telluric acid react to form silver telluride, and polyacrylonitrile is carbonized into a carbon carrier material, and finally the target product, silver telluride composite carbon nanofibers, is obtained.

[0048] Example 3

[0049] A method for preparing transition metal telluride composite carbon nanofibers, specifically nickel telluride composite carbon nanofibers, comprises the following steps:

[0050] S1. Preparation of electrospinning solution

[0051] 0.7 g of polyacrylonitrile, 0.3 mmol of nickel chloride hexahydrate, and 0.6 mmol of telluric acid were dissolved in 6 mL of N,N-dimethylformamide to prepare an electrospinning solution;

[0052] S2. Preparation of nickel chloride-telluric acid doped polyacrylonitrile nanofibers

[0053] The electrospinning solution is loaded into the syringe of the electrospinning device, and the electrospinning solution is stretched and extended in the air by electrospinning under the action of a high voltage electric field, and finally solidified into nanofibers on the aluminum foil of the receiving device. After the electrospinning is completed, the nanofiber membrane is placed in a drying oven for vacuum drying to obtain nickel chloride-telluric acid doped polyacrylonitrile nanofibers. Among them, the static voltage is 13kV, the extrusion rate of the electrospinning solution is 0.25mL / h, the receiving distance is 20cm, and the rolling speed of the receiving roller is 90r / min.

[0054] S3. Preparation of nickel telluride composite carbon nanofibers:

[0055] The nickel chloride-telluric acid doped polyacrylonitrile nanofibers are placed in a porcelain boat and placed in a tubular furnace. They are first pre-oxidized at 290°C for 2 hours in an air atmosphere, and then calcined at 800°C for 1.5 hours in an inert atmosphere. During the calcination process, nickel chloride and telluric acid react to form nickel telluride, and polyacrylonitrile is carbonized into a carbon carrier material. Finally, the target product, nickel telluride composite carbon nanofibers, is obtained.

[0056] Example 4

[0057] A method for preparing a transition metal telluride composite carbon nanofiber, specifically a copper telluride composite carbon nanofiber, comprising the following steps:

[0058] S1. Preparation of electrospinning solution

[0059] 1.5 g of polyacrylonitrile, 0.8 mmol of cupric chloride dihydrate, and 1.6 mmol of telluric acid were dissolved in 12 mL of N,N-dimethylformamide to prepare an electrospinning solution;

[0060] S2. Preparation of copper chloride-telluric acid doped polyacrylonitrile nanofibers

[0061] The electrospinning solution is loaded into the syringe of the electrospinning device, and the electrospinning solution is stretched and extended in the air by electrospinning under the action of a high voltage electric field, and finally solidified into nanofibers on the aluminum foil of the receiving device. After the electrospinning is completed, the nanofiber membrane is placed in a drying oven for vacuum drying to obtain copper chloride-telluric acid doped polyacrylonitrile nanofibers. Among them, the static voltage is 13kV, the extrusion rate of the electrospinning solution is 0.25mL / h, the receiving distance is 20cm, and the rolling speed of the receiving roller is 90r / min.

[0062] S3. Preparation of copper telluride composite carbon nanofibers:

[0063] The copper chloride-telluric acid doped polyacrylonitrile nanofibers are placed in a porcelain boat and placed in a tubular furnace. They are first pre-oxidized at 250°C for 2 hours in an air atmosphere, and then calcined at 1000°C for 1 hour in an inert atmosphere. During the calcination process, copper chloride and telluric acid react to form copper telluride, and polyacrylonitrile is carbonized to form a carbon carrier material. Finally, the target product, copper telluride composite carbon nanofibers, is obtained.

[0064] The transition metal telluride (ruthenium telluride, silver telluride, nickel telluride and copper telluride) composite carbon nanofibers prepared in Examples 1-4 were characterized by XRD. The characterization results are as follows: Figure 1-4 shown.

[0065] Depend on Figure 1-4 The results show that the diffraction peaks of ruthenium telluride composite carbon nanofibers, silver telluride composite carbon nanofibers, nickel telluride composite carbon nanofibers and copper telluride composite carbon nanofibers are respectively 2 (JCPDS No.73-1679), Ag 2 Te(JCPDS No.73-1755), NiTe 2 (JCPDS No.65-3377) and Cu 7 Te 4 (JCPDS No.65-2057) corresponds to the XRD standard card, indicating that the products are all pure phase transition metal tellurides (ruthenium telluride, silver telluride, nickel telluride and copper telluride).

[0066] The morphology of the ruthenium telluride composite carbon nanofibers prepared in Example 1 was characterized, and the SEM and TEM images of the ruthenium telluride composite carbon nanofibers were obtained, as shown in FIG. Figure 5 and Figure 6 shown.

[0067] Depend on Figure 5 The results show that the size of ruthenium telluride composite carbon nanofibers is 200-300nm, and the fibers are stacked on each other to form a large number of pores. This non-woven fiber structure is conducive to the penetration of electrolyte and the escape of gas.

[0068] Depend on Figure 6 The results show that a large number of ruthenium telluride nanoparticles are uniformly loaded on the surface of the carbon support. This supported catalyst can expose a large number of catalytic active sites, and the carbon support improves the electrocatalytic stability of the ruthenium telluride nanoparticles and provides a fast electron transfer channel. The above characterization data proves that transition metal telluride composite carbon nanofibers (ruthenium telluride composite carbon nanofibers, silver telluride composite carbon nanofibers, nickel telluride composite carbon nanofibers, and copper telluride composite carbon nanofibers) have been successfully prepared.

[0069] Test Example 1

[0070] The transition metal telluride composite carbon nanofibers (ruthenium telluride composite carbon nanofibers, silver telluride composite carbon nanofibers, nickel telluride composite carbon nanofibers, and copper telluride composite carbon nanofibers) prepared in Examples 1-4 are used as hydrogen evolution catalysts in the electrolysis of water to produce hydrogen, and the specific steps are as follows:

[0071] Preparation of working electrode: 4 mg of transition metal telluride composite carbon nanofibers and 80 μL of 5 wt% Nafion solution were dispersed in 1 mL of deionized water / ethanol mixed solution (v / v = 4 / 1) to form a uniform catalyst suspension; 5 μL of the suspension was dropped on the surface of a glassy carbon electrode (3 mm in diameter) and dried at room temperature to obtain an electrocatalyst loading of approximately 0.265 mg cm -2 working electrode.

[0072] The electrocatalytic hydrogen evolution performance of the catalyst was tested in a standard three-electrode cell, with a glassy carbon electrode loaded with the catalyst as the working electrode, a carbon rod as the counter electrode, and a saturated calomel electrode as the reference electrode. 2 SO 4 The electrocatalytic hydrogen evolution performance (LSV) test was carried out in 1M KOH solution, and the scanning rate of the LSV test was 2mV·s -1 , the experimental test temperature is 22±2℃. For specific results, see Figure 7 and Figure 8 .

[0073] Depend on Figure 7 and Figure 8 The results show that whether it is at 0.5MH 2 SO 4 In the 1M KOH solution, the ruthenium telluride composite carbon nanofiber has the highest electrocatalytic hydrogen evolution activity, followed by the copper telluride composite carbon nanofiber, the silver telluride composite carbon nanofiber and the nickel telluride composite carbon nanofiber. 2 SO 4 solution and 1M KOH solution, generating 10 mA cm -2 The catalytic current density of hydrogen evolution is 24mV and 18mV respectively. In addition, the results of constant potential electrolysis test show that the ruthenium telluride composite carbon nanofibers have a high current density of 0.5MH 2 SO 4 The transition metal telluride composite carbon nanofiber has good electrocatalytic stability in both 1M solution and 1M KOH solution. Compared with commercial Pt / C catalyst, the transition metal telluride composite carbon nanofiber has lower price cost and good structural advantages. Therefore, the transition metal telluride composite carbon nanofiber provided by the present invention can be used as a hydrogen evolution catalyst with excellent performance in the electrolysis of water to produce hydrogen.

[0074] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.

Claims

1. A method for preparing transition metal telluride composite carbon nanofibers, characterized in that: The following steps are involved: S1. Preparation of electrospinning solution: Polyacrylonitrile, transition metal salt and telluric acid are dissolved in N,N-dimethylformamide to prepare an electrospinning solution; S2. Preparation of transition metal salt-telluric acid doped polyacrylonitrile nanofibers: The electrospinning solution prepared in step S1 is transferred to an electrospinning device, and transition metal salt-telluric acid-doped polyacrylonitrile nanofibers are obtained by electrospinning. S3. Preparation of transition metal telluride composite carbon nanofibers: The transition metal salt-telluric acid doped polyacrylonitrile nanofiber is placed in a tube furnace for pre-oxidation, and then heated and calcined to obtain the transition metal telluride composite carbon nanofiber.

2. The method for preparing transition metal telluride composite carbon nanofibers according to claim 1, wherein: In step S1, the ratio of the transition metal salt, telluric acid, N,N-dimethylformamide, and polyacrylonitrile is 0.3-0.8 mmol: 0.6-1.6 mmol: 6-12 mL: 0.7-1.5 g.

3. The method for preparing transition metal telluride composite carbon nanofibers according to claim 1, wherein: In step S2, the electrospinning conditions are: static voltage of 10-18 kV, extrusion rate of electrospinning solution of 0.1-0.5 mL / h, receiving distance of 10-30 cm, and rolling speed of receiving roller of 60-200 r / min.

4. The method for preparing transition metal telluride composite carbon nanofibers according to claim 1, wherein: In step S3, the pre-oxidation is carried out in an air atmosphere, the pre-oxidation temperature is 250-300° C., and the pre-oxidation time is 0.5-2 hours.

5. The method for preparing transition metal telluride composite carbon nanofibers according to claim 1, wherein: In step S3, the calcination is carried out in an inert atmosphere, the calcination temperature is 700-1000° C., and the calcination time is 1-3 hours.

6. A transition metal telluride composite carbon nanofiber prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the transition metal telluride composite carbon nanofiber according to claim 6 as a catalyst in hydrogen production by water electrolysis.