A method for recycling magnesium-containing mixed waste brick slag

By mixing the crushed magnesium-containing mixed waste brick slag with dust removal powder and light-burned dolomite powder to make magnesium carbon balls, which are used as slag splashing and furnace protection materials in steelmaking plants. This solves the problem of waste brick slag occupying space and pollution, and achieves It achieves resource recycling and production cost reduction, and improves the refractoriness of the slag splash layer and the utilization rate of the converter.

CN116854492BActive Publication Date: 2024-10-15HUNAN XIANGGANG RUITAI TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310916680.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-25
Publication Date
2024-10-15
Estimated Expiration
2043-07-25

AI Technical Summary

Technical Problem

The magnesium-containing mixed waste brick slag discarded by the refractory industry has not been properly utilized, resulting in site occupation and environmental pollution. There is no specific treatment method in the existing technology.

Method used

After collecting and crushing magnesium-containing mixed waste brick slag, sieving and mixing dust removal powder, light-burned dolomite powder and bentonite are made into pellets. After cooling, magnesium carbon pellets are obtained and used in steelmaking plants. Slag splashing protects the furnace charge.

Benefits of technology

It achieves efficient recycling of waste brick slag, reduces environmental pollution and production costs, and at the same time improves the refractoriness of the slag splash layer and the utilization rate of the converter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004357194750000051
    Figure BDA0004357194750000051
  • Figure BDA0004357194750000062
    Figure BDA0004357194750000062
  • Figure BDA0004357194750000071
    Figure BDA0004357194750000071
Patent Text Reader

Abstract

The present application discloses a method for recycling magnesium-containing mixed waste brick slag, comprising the following steps: S1, collecting magnesium-containing mixed waste brick slag, crushing and sieving; S2, mixing the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieved material in the following weight parts: 60-80 weight parts of magnesium-containing mixed waste brick slag, 10-20 weight parts of dust removal powder, 20-35 weight parts of light-burned dolomite powder, 1-2 weight parts of bentonite, to obtain a mixture; S3, making the mixture obtained in step S2 into pellets, and cooling the pellets after keeping them warm for a period of time under a certain stability to obtain magnesium-carbon balls; S4, using the magnesium-carbon balls obtained in step S3 as slag splashing furnace protection materials in steel plants. The present application can maximize the recycling of magnesium-containing mixed waste brick slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of waste recycling in the refractory industry, and in particular to a method for recycling magnesium-containing mixed waste brick slag. Background Art

[0002] In order to save resources and reduce production and manufacturing costs, the refractory industry will choose to dismantle and centrally recycle all the ladles, converters, electric furnaces and RH bricks after they have served in the steel mill. However, during the dismantling process of the brick dismantling machine and during the transportation of recycling, the bricks will be broken due to collisions, leaving only a part. At the same time, when these bricks are recycled to the yard, they are all exposed to water for a long time in the open air. In addition, they are piled up outdoors for a long time in the wind and rain, and a series of chemical reactions will occur on the surface of the bricks, resulting in natural peeling and powdering of the bricks. Over time, these residues will accumulate more and more, and due to limited space and the large number of brick varieties piled together, if accumulated over the years, these magnesium-containing waste brick slags have not been properly utilized, occupying the site and polluting the environment. There is no research report on the treatment of magnesium-containing waste brick slag recycled from steel mills in the prior art.

[0003] How to realize the recycling of magnesium-containing mixed waste brick slag is a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for recycling magnesium-containing mixed waste brick slag, which can maximize the recycling of magnesium-containing mixed waste brick slag.

[0005] The technical solution provided by the present invention is as follows:

[0006] A method for recycling magnesium-containing mixed waste brick slag comprises the following steps:

[0007] S1, collecting the magnesium-containing mixed waste brick slag, crushing it and screening it;

[0008] S2, the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieve are uniformly mixed according to the following weight parts: 60-80 weight parts of magnesium-containing mixed waste brick slag, 10-20 weight parts of dust removal powder, 20-35 weight parts of light-burned dolomite powder, 1-2 weight parts of bentonite, to obtain a mixture;

[0009] S3, making the mixture obtained in step S2 into pellets, and keeping the pellets warm for a period of time under a certain stability and then cooling them to obtain magnesium carbon balls;

[0010] S4, using the magnesium carbon balls prepared in step S3 as slag splashing furnace protection materials in steel plants.

[0011] Preferably, the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieve are evenly mixed according to the following weight parts: 65-70 weight parts of magnesium-containing mixed waste brick slag, 15-18 weight parts of dust removal powder, 25-30 weight parts of light-burned dolomite powder and 1-2 weight parts of bentonite.

[0012] Preferably, in step S1, the magnesium-containing mixed waste brick slag is firstly sorted after being crushed to obtain magnesium-containing waste brick slag with higher purity, and then sieved.

[0013] Preferably, the sorting process is carried out by utilizing the difference in specific gravity of different bricks, and the impurities with smaller specific gravity and the waste magnesia-chrome brick slag, waste magnesia-carbon brick slag and waste aluminum-magnesia-carbon brick slag with larger specific gravity are separated in layers by utilizing the different settling speeds in the medium.

[0014] Preferably, the particle size of the magnesium-containing mixed waste brick slag under the sieve in step S2 is less than or equal to 3 mm;

[0015] The mixing time in step S2 is 10-15 min.

[0016] Preferably, the diameter of the pellets in step S3 is 20-50 mm.

[0017] Preferably, in step S3, the pellets are kept warm at a temperature of 200-250° C. for a time of 10-12 hours.

[0018] Preferably, the weight content characteristics of the components in the magnesium-containing mixed waste brick slag in step S2 are: MgO≥65%, CaO≥2%, SiO2≤8%, Al2O3≤15%, C≥10%, and other impurities≤1%.

[0019] Preferably, the dust powder in step S2 is collected from a steel plant workshop.

[0020] Preferably, the use process of magnesium carbon balls in step S4 is: after the steelmaking converter has finished producing steel, magnesium carbon balls are added into the furnace from the high-level silo, the feeding time is 150s-180s, and 300-800 kg of magnesium carbon balls are added to each furnace. During the addition of magnesium carbon balls, high-pressure nitrogen is blown into the furnace to perform slag splashing and furnace protection operations.

[0021] The present application has the following advantages over the prior art:

[0022] The method for recycling magnesium-containing mixed waste brick slag of the present invention utilizes waste brick slag and workshop dust removal powder discarded in the refractory industry as the main raw materials. The use of waste brick slag powder and workshop dust removal powder in magnesium-carbon ball products not only realizes the recycling of waste resources, reduces the company's annual waste discharge costs, solves land occupation and environmental pollution problems, but also reduces environmental pollution and reduces the production cost of the product.

[0023] The magnesium carbon balls prepared in the present application have appropriate magnesium oxide content and viscosity and are used for slag splashing furnace protection operations. They can improve the refractoriness of the slag splashing layer, improve the effect of slag splashing furnace protection, strengthen the protection of the converter lining material, reduce the use of converter supplementary materials, improve the utilization rate of the converter, and further extend the life of the converter.

[0024] It is further preferred that the magnesium-containing mixed waste brick slag in step S1 is first sorted after crushing to obtain magnesium-containing waste brick slag with high purity, and then screened. It is more preferred that the sorting process is carried out using the difference in specific gravity of different bricks, and the impurities with smaller specific gravity and the waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated and sorted in layers by using the different sedimentation rates in the medium. By utilizing the differences in density, particle size and specific gravity of various bricks, with the help of fluid dynamics and various mechanical forces, suitable loose spreading and separation conditions are created, thereby obtaining high-purity magnesium-containing mixed waste brick slag with different densities and different particle sizes, which is simple to produce, low in cost and easy to use. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0026] The embodiment of the present invention provides a method for recycling magnesium-containing mixed waste brick slag, comprising the following steps:

[0027] S1, collecting the magnesium-containing mixed waste brick slag, crushing it and screening it;

[0028] S2, the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieve are uniformly mixed according to the following weight parts: 60-80 weight parts of magnesium-containing mixed waste brick slag, 10-20 weight parts of dust removal powder, 20-35 weight parts of light-burned dolomite powder, 1-2 weight parts of bentonite, to obtain a mixture;

[0029] S3, making the mixture obtained in step S2 into pellets, and keeping the pellets warm for a period of time under a certain stability and then cooling them to obtain magnesium carbon balls;

[0030] S4, using the magnesium carbon balls prepared in step S3 as slag splashing furnace protection materials in steel plants.

[0031] Preferably, the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieve are evenly mixed according to the following weight parts: 65-70 weight parts of magnesium-containing mixed waste brick slag, 15-18 weight parts of dust removal powder, 25-30 weight parts of light-burned dolomite powder and 1-2 weight parts of bentonite.

[0032] Preferably, in step S1, the magnesium-containing mixed waste brick slag is firstly sorted after being crushed to obtain magnesium-containing waste brick slag with higher purity, and then sieved.

[0033] In this embodiment, the sorting process is carried out by utilizing the difference in specific gravity of different bricks, and the impurities with smaller specific gravity and the waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated and sorted in layers by utilizing the different settling speeds in the medium.

[0034] In this embodiment, the particle size of the magnesium-containing mixed waste brick slag under the sieve in step S2 is less than or equal to 3 mm;

[0035] The mixing time in step S2 is 10-15 min.

[0036] In this embodiment, the diameter of the pellets in step S3 is 20-50 mm.

[0037] In this embodiment, the pellets are kept warm at a temperature of 200-250° C. for a time of 10-12 hours in step S3.

[0038] In this embodiment, the weight content characteristics of the components in the magnesium-containing mixed waste brick slag in step S2 are: MgO≥65%, CaO≥2%, SiO2≤8%, Al2O3≤15%, C≥10%, and other impurities≤1%.

[0039] In this embodiment, the dust powder in step S2 is collected from a steel plant workshop.

[0040] In this embodiment, the use process of magnesium carbon balls in step S4 is as follows: after the steelmaking converter has finished producing steel, magnesium carbon balls are added into the furnace from the high-level silo. The feeding time is 150s-180s, and 300-800 kg of magnesium carbon balls are added to each furnace. During the addition of magnesium carbon balls, high-pressure nitrogen is blown into the furnace to perform slag splashing and furnace protection operations.

[0041] Measured data of raw materials used in Examples 1-3:

[0042] Waste brick slag powder MgO CaO <![CDATA[SiO2]]> C <![CDATA[Al2O3]]> content 70% 2.00% 5.00% 13% 10%

[0043] Lightly burned dolomite powder MgO <![CDATA[SiO2]]> content 30% 2.00%

[0044] Workshop dust removal powder MgO <![CDATA[SiO2]]> C content 50% 3.00% 45%

[0045] Embodiment 1:

[0046] Collect all the waste magnesium-containing mixed waste brick slag, use the existing efficient and intelligent gravity separation equipment to separate by using the difference in specific gravity of different bricks, and then enter the gravity separation equipment for separation after crushing and fine grinding. The impurities with smaller specific gravity and waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated by different sedimentation rates in the medium to obtain high-purity magnesium-containing waste brick slag, and the proportion of light-burned dolomite powder, dust removal powder and bentonite is 65 parts by weight, 30 parts by weight, 15 parts by weight and 1 part by weight. According to the technical formula of raw materials required by the process, add them to the efficient mixing mill and mix for 10 minutes. Then use the ball press to press them into the specified 20-50mm specification spheres, and then send them to the drying kiln, keep them in the drying kiln at 200℃-250℃ for 10-12 hours, and then screen them out of the kiln to ensure that the discharge meets the 20-50mm specification requirements. After natural cooling, they can be packed into ton bags for distribution to the steel mill.

[0047] Embodiment 2:

[0048] Collect all the waste magnesium-containing mixed waste brick slag, use the existing efficient and intelligent gravity separation equipment to separate by using the difference in specific gravity of different bricks, and then enter the gravity separation equipment for separation after crushing and fine grinding. The impurities with smaller specific gravity and waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated by different sedimentation rates in the medium to obtain high-purity magnesium-containing waste brick slag, and add light-burned dolomite powder, workshop dust removal powder, and bentonite in the proportion of 70 parts by weight, 25 parts by weight, 15 parts by weight, and 1 part by weight. According to the technical formula of the raw materials required by the process, add them to the efficient mixing mill and mix for 10 minutes. Then use the ball press to press into the specified 20-50mm specification sphere, and then send it to the drying kiln, keep it in the 200-250℃ drying kiln for 10-12 hours, and then screen it to ensure that the discharge meets the 20-50mm specification requirements. After natural cooling, it can be packed into ton bags and distributed to the steel mill for use.

[0049] Embodiment 3:

[0050] Collect all the waste magnesium-containing mixed waste brick slag, use the existing efficient and intelligent gravity separation equipment to separate by using the difference in specific gravity of different bricks, and then enter the gravity separation equipment for separation after crushing and fine grinding. The impurities with smaller specific gravity and waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated by different sedimentation rates in the medium to obtain high-purity magnesium-containing waste brick slag, and add light-burned dolomite powder, workshop dust removal powder, and bentonite in the proportion of 70 parts by weight, 25 parts by weight, 15 parts by weight, and 1 part by weight. According to the technical formula of the raw materials required by the process, add them to the efficient mixing mill and mix for 15 minutes. Then use the ball press to press into the specified 20-50mm specification sphere, and then send it to the drying kiln, keep it in the 200-250℃ drying kiln for 10-12 hours, and then screen it to ensure that the discharge meets the 20-50mm specification requirements. After natural cooling, it can be packed into ton bags and distributed to the steel mill for use.

[0051] The chemical composition analysis (weight percentage) of the magnesium carbon spheres prepared in Example 3 is performed, and the results are shown in Table 1 below.

[0052] Table 1 Chemical composition analysis results of magnesium carbon balls obtained in Examples 1-3

[0053]

[0054]

[0055] The analysis results in Table 1 above indicate that the chemical composition of the magnesium-carbon balls prepared using waste magnesium-containing waste brick slag powder as raw material meets the requirements of slag splashing furnace protection operations.

[0056] The magnesium carbon balls prepared in Examples 1-3 were subjected to drop strength tests (using a testing instrument to let the magnesium carbon balls prepared in Examples fall freely from a height of 0.5 m onto a 10 mm thick steel plate, and the drop strength (m) was calculated from the data measured by the instrument) and compressive strength tests. Ten sample balls were taken for each test, and the average value was taken. The results are shown in Table 2 below.

[0057] Table 2 Results of drop test and compressive strength test of magnesium carbon balls obtained in Examples 1-3

[0058] Example Drop strength (m) Compressive strength (KN / piece) Example 1 4.2 4.8 Example 2 5.3 6.5 Example 3 6.6 7.8

[0059] The national standard requirement for drop strength is that the concrete floor should not break when it falls freely from a height of 3m.

[0060] The test results in Table 2 above indicate that the magnesium carbon balls prepared in Examples 1-3 have high mechanical strength and are sufficient to withstand the bumps and shocks during transportation.

[0061] The magnesium carbon balls prepared in Example 3 are used as slag splashing furnace protection materials to modify the converter slag, wherein the smelting steel type is HRB400. After the 150-ton steelmaking converter is finished, the feeding time is controlled to be 2 minutes and 30 seconds to 3 minutes for lower gun blowing, and the material is added from the high-level silo, and each furnace is added at 300-800 / kg, and high-pressure nitrogen is blown into the furnace for slag splashing furnace protection operations, mainly using magnesium and carbon in magnesium carbon bricks to adjust the viscosity of steel slag and participate in the deoxidation reaction at the same time, optimizing the slag splashing furnace protection process. The steelmaking converter was tested on site using 16 furnaces, and the effect was good and could meet the steelmaking process requirements. The slag composition before and after the modification is shown in Table 3 below.

[0062] Table 3 Slag composition before and after converter slag modification

[0063]

[0064]

[0065] The results of the above Table 3 show that the magnesium carbon balls in Example 3 can effectively increase the magnesium oxide content of the slag and reduce the FeO content. At the same time, the dephosphorization efficiency is improved, the consumption of lime and dolomite is significantly reduced, the slag volume is also reduced, and the composition control is normal. The viscosity of the slag is also improved, so that the slag viscosity is moderate. After the slag splashing is completed, the furnace lining condition is checked. The slag hanging effect is good, and the slag splashing effect is improved. After steel is tapped, it is added to the converter, which has a significant effect on the rapid thickening of the slag, and improves the viscosity of the slag and the effect of slag splashing to protect the furnace, and reduces the time of slag splashing to protect the furnace; because the magnesium carbon balls prepared in Example 3 contain carbon, they can quickly neutralize the iron oxide in the slag, improve the slag splashing effect, and protect the furnace lining. At the same time, the slag splashing time is also reduced, reducing 20-30s / furnace, and the amount of high-pressure nitrogen can also be reduced; the magnesium oxide content of the final slag is increased, the lining erosion is reduced, and the furnace lining bricks are protected.

[0066] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for recycling magnesium-containing mixed waste brick slag, characterized in that: The steps include: S1, collecting the magnesium-containing mixed waste brick slag, crushing it and screening it; S2, the magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite of the sieve are uniformly mixed according to the following weight parts: 60-80 weight parts of magnesium-containing mixed waste brick slag, 10-20 weight parts of dust removal powder, 20-35 weight parts of light-burned dolomite powder, and 1-2 weight parts of bentonite to obtain a mixture, wherein the magnesium-containing mixed waste brick slag includes waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag, and the weight content of the components in the magnesium-containing mixed waste brick slag is characterized by: MgO≥65%, CaO≥2%, SiO2≤8%, Al2O3≤15%, C≥10%, and other impurities≤1%; the dust removal powder is collected from the workshop of the steel plant, and the chemical components of the dust removal powder include MgO 50%, SiO23%, and C 45%; S3, making the mixture obtained in step S2 into pellets, and keeping the pellets warm for a period of time under a certain stability and then cooling them to obtain magnesium carbon balls; S4, using the magnesium carbon balls prepared in step S3 as slag splashing furnace protection materials in steel plants.

2. The method for recycling magnesium-containing mixed waste brick slag according to claim 1, characterized in that: The sieved magnesium-containing mixed waste brick slag, dust removal powder, light-burned dolomite powder and bentonite are uniformly mixed according to the following weight parts: 65-70 weight parts of magnesium-containing mixed waste brick slag, 15-18 weight parts of dust removal powder, 25-30 weight parts of light-burned dolomite powder and 1-2 weight parts of bentonite.

3. The method for recycling magnesium-containing mixed waste brick slag according to claim 1, characterized in that: In the step S1, the magnesium-containing mixed waste brick slag is firstly sorted after being crushed to obtain magnesium-containing waste brick slag with higher purity, and then sieved.

4. The method for recycling magnesium-containing mixed waste brick slag according to claim 3, characterized in that: The sorting process is carried out by utilizing the difference in specific gravity of different bricks, and the impurities with smaller specific gravity and the waste magnesium-chrome brick slag, waste magnesium-carbon brick slag and waste aluminum-magnesium-carbon brick slag with larger specific gravity are separated and sorted in layers by utilizing the different settling speeds in the medium.

5. The method for recycling magnesium-containing mixed waste brick slag according to claim 1, characterized in that: The particle size of the magnesium-containing mixed waste brick slag under the sieve in step S2 is less than or equal to 3 mm; The mixing time in step S2 is 10-15 min.

6. The method for recycling magnesium-containing mixed waste brick slag according to any one of claims 1 to 5, characterized in that: The diameter of the pellets in step S3 is 20-50 mm.

7. The method for recycling magnesium-containing mixed waste brick slag according to any one of claims 1 to 5, characterized in that: In step S3, the pellets are kept at a temperature of 200-250° C. for a time of 10-12 hours.

8. The method for recycling magnesium-containing mixed waste brick slag according to any one of claims 1 to 5, characterized in that: The use process of the magnesium carbon balls in step S4 is as follows: after the steelmaking converter has finished producing steel, magnesium carbon balls are added into the furnace from the high-level silo. The feeding time is 150s-180s, and 300-800 kg of magnesium carbon balls are added to each furnace. During the addition of the magnesium carbon balls, high-pressure nitrogen is blown into the furnace to perform slag splashing and furnace protection operations.

Citation Information

Patent Citations

  • Energy-saving environmentally-friendly converter slag splashing protecting charging and production process thereof

    CN102787204A

  • Resource utilization method of waste magnesia powder after treating oriented silicon steel

    CN104099469A

  • Caustic-calcined magnesia ball prepared by regenerating used converter magnesia brick

    CN104480247A

  • Slag-splashing lining protection material regenerated by used magnesia carbon brick for converter

    CN104498665A

  • Final slag conditioning agent for semisteel smelting converter slag splashing protecting furnace and using method thereof