A 6005A aluminum alloy grain boundary etching solution

By using a corrosive solution of 1-3% hydrofluoric acid, 7-10% nitric acid, and 30% hydrochloric acid in combination with specific steps to corrode 6005A aluminum alloy, the problem of difficulty in clearly observing the grain morphology in the existing technology was solved and achieved Low-cost and efficient grain boundary observation effect.

CN116855945BActive Publication Date: 2024-10-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310806336.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-03
Publication Date
2024-10-15
Estimated Expiration
2043-07-03

AI Technical Summary

Technical Problem

Existing methods are difficult to clearly observe the grain morphology and size of 6005A aluminum alloy. They are also costly, time-consuming and cumbersome, and cannot effectively solve the observation difficulties caused by its high corrosion resistance.

Method used

The 6005A aluminum alloy is corroded using a corrosive solution of 1-3% hydrofluoric acid, 7-10% nitric acid, and 30% hydrochloric acid. It is combined with electrolytic polishing and polarization treatment. Through water bath heating and rapid rinsing steps, the crystal can be clearly observed under a microscope. boundary.

Benefits of technology

It achieves clear observation of the grain boundaries of 6005A aluminum alloy, reducing time and economic costs. The corrosion process is stable, the requirements for observation equipment are low, and the operation is simple and convenient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004318657910000011
    Figure HDA0004318657910000011
  • Figure HDA0004318657910000012
    Figure HDA0004318657910000012
  • Figure HDA0004318657910000021
    Figure HDA0004318657910000021
Patent Text Reader

Abstract

The invention discloses a 6005A aluminum alloy grain boundary etching liquid. The components and volume percentages of the 6005A aluminum alloy grain boundary etching liquid are as follows: 1-3% hydrofluoric acid, 7-10% nitric acid, 30% hydrochloric acid, and the balance is water. The etching liquid of the invention is used to etch the 6005A aluminum alloy, which has low equipment requirements, simple operation, and cost saving, and can clearly observe the grain boundaries of the aluminum alloy. The invention is suitable for studying the grain morphology, grain size, microstructure performance, and the like of the 6005A aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy metallographic corrosion, and in particular relates to a 6005A aluminum alloy grain boundary corrosion liquid. Background Art

[0002] Among the 6XXX series aluminum alloys, 6005A aluminum alloy has medium strength and is a heat-treatable Al-Mg-Si series aluminum alloy. It is widely used in high-speed trains, automobiles, and shipbuilding industries due to its excellent formability, corrosion resistance, good weldability, and suitable economy.

[0003] The grain size and morphology of aluminum alloy have a great influence on the performance of the alloy, so it is of substantial significance to be able to clearly observe the grain boundaries of aluminum alloy. The general aluminum alloy can be observed under a microscope after being corroded by Keller reagent, but 6005A aluminum alloy has strong corrosion resistance. After being corroded by Keller reagent, the morphology and size of the grains cannot be clearly observed under a microscope. At present, the methods for observing the grain morphology and grain size of aluminum alloy materials include electrolytic polishing + polarizing treatment and EBSD (electron backscatter diffraction), but these observation methods are costly, time-consuming, cumbersome and inefficient. Therefore, it is very important to explore a simple, fast and effective 6005A aluminum alloy grain boundary etching solution. Summary of the invention

[0004] Based on the deficiencies of the existing problems, the present invention provides a 6005A aluminum alloy grain boundary etching solution. The grain boundary etching solution provided by the present invention is used to corrode the metallographic structure of the 6005A aluminum alloy, so that the obtained grain boundaries are clearly visible, the time cost and the economic cost are low, and the corrosion process is stable.

[0005] The technical solution of the present invention is:

[0006] The invention discloses a 6005A aluminum alloy grain boundary etching liquid, the components and volume percentages of which are: 1-3% hydrofluoric acid, 7-10% nitric acid, 30% hydrochloric acid, and the balance is water.

[0007] The mass concentrations of the hydrofluoric acid, nitric acid and hydrochloric acid are 40%, 63% and 36-38% respectively.

[0008] The method for corroding 6005A aluminum alloy using the above-mentioned corrosive solution has the following specific steps:

[0009] (1) Preparation of metallographic specimens: The aluminum alloy specimens were mounted and removed after being cooled and solidified;

[0010] (2) Grinding: Grind the prepared metallographic specimen with sandpaper from low to high grit;

[0011] (3) Polishing: Polish the polished sample with a grinding and polishing machine;

[0012] (4) Corrosion: Pour the corrosive solution into a container, place it in a water bath and heat it to 55° C., clean and dry the polished sample, and immerse the polished surface in the corrosive solution and corrode it in a water bath for 30 seconds to 40 seconds;

[0013] (5) Rinse: Rinse the polished surface after corrosion with distilled water, then clean it with anhydrous ethanol, and use a hair dryer to quickly dry it;

[0014] (6) Metallographic inspection: Place the corroded metallographic sample under a metallographic microscope to observe the metallographic structure.

[0015] Furthermore, in the step (1), the aluminum alloy sample is embedded using epoxy resin powder and epoxy resin curing agent, and the embedding temperature is room temperature and the time is 20 minutes.

[0016] Furthermore, in the step (2), the mesh sizes of sandpaper are 400 mesh, 600 mesh, 1000 mesh, 1500 mesh, 2000 mesh, 3000 mesh, 5000 mesh and 7000 mesh, respectively, and the sanding is performed under running water.

[0017] Furthermore, in the step (3), a silk polishing cloth and a diamond polishing spray with a particle size of 0.5 μm are first used for rough polishing, and after the polishing marks are in the same direction, a flocked polishing cloth and a diamond polishing spray with a particle size of 0.25 μm are used for fine polishing until the surface has a mirror-like gloss and there are no polishing marks when observed under an optical microscope.

[0018] Beneficial effects of the present invention:

[0019] The etching solution of the invention has good etching effect on 6005A aluminum alloy, the grain boundary and the grain size are clearly visible, the requirement for observation equipment is low, the etching operation is simple and convenient, the chemical reagents for preparing the grain boundary etching solution are all commonly used reagents, which are easy to obtain and low in cost, and are conducive to the performance research of 6005A aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a metallographic structure photograph obtained by etching in Example 4;

[0021] Figure 2 This is a metallographic structure photograph obtained by etching in Example 5;

[0022] Figure 3 This is a metallographic structure photograph of the comparative example 1. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further explained in detail below with reference to the accompanying drawings.

[0024] Example 1

[0025] A 6005A aluminum alloy grain boundary etching solution is prepared by first adding 60 mL of water into a beaker, then sequentially adding 1 mL of hydrofluoric acid, 7 mL of nitric acid and 30 mL of hydrochloric acid, and then adding water to prepare 100 mL of etching solution, wherein the mass concentrations of the hydrofluoric acid, the nitric acid and the hydrochloric acid are 40%, 63% and 38% respectively, and the 6005A aluminum alloy grain boundary etching solution with similar performance is obtained.

[0026] Example 2

[0027] The invention discloses a 6005A aluminum alloy grain boundary etching liquid. 60 mL of water is first added into a beaker, and then 3 mL of hydrofluoric acid, 10 mL of nitric acid and 30 mL of hydrochloric acid are added in sequence. Water is then added to prepare 100 mL of etching liquid. The mass concentrations of the hydrofluoric acid, the nitric acid and the hydrochloric acid are 40%, 63% and 36% respectively. The 6005A aluminum alloy grain boundary etching liquid with similar performance is obtained.

[0028] Example 3

[0029] A 6005A aluminum alloy grain boundary etching solution is prepared by first adding 60 mL of water into a beaker, then sequentially adding 2 mL of hydrofluoric acid, 8 mL of nitric acid and 30 mL of hydrochloric acid, and then adding water to prepare 100 mL of etching solution, wherein the mass concentrations of the hydrofluoric acid, the nitric acid and the hydrochloric acid are 40%, 63% and 36% respectively, and the 6005A aluminum alloy grain boundary etching solution with similar performance is obtained.

[0030] Example 4

[0031] The gold grain boundary etching solution prepared in Example 3 was used to corrode 6005A aluminum alloy, and the specific steps were as follows:

[0032] (1) Preparation of metallographic specimens: The aluminum alloy specimens were mounted and removed after being cooled and solidified;

[0033] (2) Grinding: Grind the prepared metallographic sample with sandpaper of low to high grit, i.e., 400 grit, 600 grit, 1000 grit, 1500 grit, 2000 grit, 3000 grit, 5000 grit, and 7000 grit, and grind under running water; (3) Polishing: Polish the polished sample with a grinding and polishing machine, first use a silk polishing cloth and a diamond polishing spray with a particle size of 0.5 μm for rough polishing, and then use a flocked polishing cloth and a diamond polishing spray with a particle size of 0.25 μm for fine polishing after the polishing marks are in the same direction, until the surface has a mirror gloss and there are no polishing marks under an optical microscope;

[0034] (4) Corrosion: Pour the corrosive solution into a container, place it in a water bath and heat it to 55° C., clean and dry the polished sample, and immerse the polished surface in the corrosive solution and corrode it in a water bath for 30 seconds;

[0035] (5) Rinse: Rinse the polished surface after corrosion with distilled water, then clean it with anhydrous ethanol, and use a hair dryer to quickly dry it;

[0036] (6) Metallographic inspection: Place the corroded metallographic sample under a metallographic microscope to observe the metallographic structure.

[0037] The grain boundaries obtained by etching using the above method are Figure 1 As shown, it can be observed that the grain boundaries of the alloy are clear and complete, the corrosion effect is good and easy to observe.

[0038] Example 5

[0039] The gold grain boundary etching solution prepared in Example 3 was used to corrode 6005A aluminum alloy, and the specific steps were as follows:

[0040] (1) Preparation of metallographic specimens: The aluminum alloy specimens were mounted and removed after being cooled and solidified;

[0041] (2) Grinding: Grind the prepared metallographic sample with sandpaper of low to high grit, i.e., 400 grit, 600 grit, 1000 grit, 1500 grit, 2000 grit, 3000 grit, 5000 grit, and 7000 grit, and grind under running water; (3) Polishing: Polish the polished sample with a grinding and polishing machine, first use a silk polishing cloth and a diamond polishing spray with a particle size of 0.5 μm for rough polishing, and then use a flocked polishing cloth and a diamond polishing spray with a particle size of 0.25 μm for fine polishing after the polishing marks are in the same direction, until the surface has a mirror gloss and there are no polishing marks under an optical microscope;

[0042] (4) Corrosion: Pour the corrosive solution into a container, place it in a water bath and heat it to 55° C., clean and dry the polished sample, and immerse the polished surface in the corrosive solution and corrode it in a water bath for 40 seconds;

[0043] (5) Rinse: Rinse the polished surface after corrosion with distilled water, then clean it with anhydrous ethanol, and use a hair dryer to quickly dry it;

[0044] (6) Metallographic inspection: Place the corroded metallographic sample under a metallographic microscope to observe the metallographic structure.

[0045] The grain boundaries obtained by etching using the above method are Figure 2 As shown, it can be observed that the grain boundaries of the alloy are clear and complete, the corrosion effect is good and easy to observe.

[0046] Comparative Example 1

[0047] The etching solution in the example was replaced with the commercial etching agent Keller reagent, and etching was carried out in the manner of Example 5. The obtained metallographic structure is as follows Figure 3 As shown, it can be seen that some precipitated phases of the aluminum alloy are corroded, but the grain boundaries cannot be observed, and the corrosion effect is poor.

[0048] The above specific implementation measures are only used to describe the technical solution of the present invention and are not limiting. Although the present invention has been described in detail through embodiments, ordinary technicians in the field should understand that the technical solution can be appropriately changed, modified and replaced without departing from the technical solution and spirit of the present invention. The scope of the present invention is defined by the attached claims and their equivalents.

Claims

1. A 6005A aluminum alloy grain boundary etching solution, characterized in that: Its components and volume percentages are: 1-3% hydrofluoric acid, 7-10% nitric acid, 30% hydrochloric acid, and the balance is water; The mass concentrations of hydrofluoric acid, nitric acid and hydrochloric acid are 40%, 63%, 36-38% respectively; Heat the etching solution to 55°C before use.