Vinyl acetate grafted starch and preparation method and application thereof, starch / PBAT composite material and preparation method thereof

By grafting starch with vinyl acetate as a compatibilizer, the compatibility of starch and PBAT is significantly improved, solving the problems of poor compatibility and high cost in the existing technology, and achieving complete compatibility and mechanical stability of starch/PBAT composite materials. Improved performance, suitable for food packaging field.

CN117003945BActive Publication Date: 2024-10-29WUHAN TEXTILE UNIV +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311013885.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-10-29
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

Starch has poor compatibility with PBAT materials. Existing compatibilizers have limited effects and high costs, making it difficult to achieve complete compatibility and reduce material costs.

Method used

Vinyl acetate grafted starch is used as a compatibilizer, and the compatibility of starch and PBAT is significantly improved through graft modification of gelatinized starch with vinyl acetate and initiator, and starch/PBAT is prepared through twin-screw extrusion processing. composite materials.

Benefits of technology

The complete compatibility of starch and PBAT is achieved, which reduces production costs. Vinyl acetate-grafted starch is fully biodegradable. The starch/PBAT composite material has excellent mechanical properties and is suitable for the field of food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117003945B_ABST
    Figure CN117003945B_ABST
Patent Text Reader

Abstract

The present invention provides vinyl acetate grafted starch, a preparation method and application thereof, a starch / PBAT composite material and a preparation method thereof, and relates to the technical field of polymer materials. In the present invention, starch is mixed with water for gelatinization to obtain gelatinized starch; the gelatinized starch, vinyl acetate and an initiator are mixed for grafting modification to obtain the vinyl acetate grafted starch. In the present invention, starch is used as a raw material, water is used as a solvent, and vinyl acetate is used as a grafting monomer to prepare grafted starch under the action of an initiator. The starch / PBAT system is expanded using the vinyl acetate grafted starch prepared by the present invention as a compatibilizer, which can achieve complete compatibility between starch and PBAT; and the vinyl acetate grafted starch prepared by the present invention is low in price and fully biodegradable compared to other compatibilizers, making the starch / PBAT composite material one step closer to full starch plastics, and is expected to enter the field of food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to vinyl acetate grafted starch and a preparation method and application thereof, and a starch / PBAT composite material and a preparation method thereof. Background Art

[0002] Traditional petroleum-based plastics are difficult to degrade and have a serious impact on the environment. The development and research of environmentally friendly biodegradable plastics has become one of the important directions for the future development of the plastics industry. Polybutylene terephthalate-adipate (PBAT) is a thermoplastic biodegradable material with excellent performance, high elongation and good toughness. It can be used in degradable film bags, ground films and other fields. However, PBAT itself is relatively expensive and difficult to promote and apply on a large scale. Starch, as a natural macromolecule, is widely available and inexpensive. The starch / PBAT composite material prepared by blending PBAT and starch can reduce material costs while ensuring degradation, and has good development prospects.

[0003] However, the compatibility of starch and PBAT materials is poor, and a compatibilizer needs to be added to improve the compatibility of the two. Adding a suitable compatibilizer can not only further improve the performance of the starch / PBAT composite material, but also add more starch without affecting the comprehensive performance of the composite material, thereby further reducing the cost. Commonly used compatibilizers mainly include tributyl citrate (TBC), triphenyl phosphite (TPPI), and soluble polyester (PVE). However, the compatibilization effect of these compatibilizers still needs to be improved, and starch and PBAT cannot be completely compatible; and the price is relatively high, which increases the production cost. Summary of the invention

[0004] In view of this, the object of the present invention is to provide vinyl acetate grafted starch and its preparation method and application, starch / PBAT composite material and its preparation method. The vinyl acetate grafted starch prepared by the present invention as a compatibilizer can achieve complete compatibility between starch and PBAT, and the cost is low.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing vinyl acetate grafted starch, comprising the following steps:

[0007] The starch is mixed with water for gelatinization to obtain gelatinized starch;

[0008] The gelatinized starch, vinyl acetate and an initiator are mixed for grafting modification to obtain the vinyl acetate grafted starch.

[0009] Preferably, the gelatinization temperature is 80-120°C.

[0010] Preferably, the mass ratio of starch to vinyl acetate is (0.8-1.2):(1.8-2.2).

[0011] Preferably, the initiator is ammonium cerium nitrate, and the mass of the initiator is 2.5-3.5% of the mass of starch.

[0012] Preferably, the specific operation of the graft modification comprises the following steps:

[0013] adding part of vinyl acetate and part of initiator to the gelatinized starch in sequence, and then simultaneously adding the remaining vinyl acetate and the remaining initiator dropwise to the obtained mixture;

[0014] The part of vinyl acetate is 1 / 3 of the total mass of vinyl acetate, and the part of initiator is 1 / 3 of the total mass of initiator; the dropping speed of the remaining vinyl acetate is 3s / drop, and the dropping speed of the remaining initiator is 20s / drop.

[0015] Preferably, the temperature of the graft modification is 40-60° C., the time is 3-5 hours, and the time of the graft modification is calculated from the completion of the addition of the part of vinyl acetate; the graft modification is carried out in a nitrogen atmosphere.

[0016] The present invention provides vinyl acetate grafted starch prepared by the preparation method described in the above technical scheme.

[0017] The present invention provides the use of the vinyl acetate grafted starch described in the above technical solution as a compatibilizer in the preparation of a starch / PBAT composite material.

[0018] The present invention provides a starch / PBAT composite material, comprising the following raw materials in parts by weight: 1 part of starch, 0.25-0.5 parts of glycerol, 0.3-0.6 parts of a compatibilizer, and 0.8-1.2 parts of PBAT; the compatibilizer is the vinyl acetate grafted starch described in the above technical solution.

[0019] The present invention provides a method for preparing the starch / PBAT composite material described in the above technical solution, comprising the following steps:

[0020] The starch, glycerol and a compatibilizer are mixed and pre-plasticized, and the obtained mixture is subjected to twin-screw extrusion processing with PBAT to obtain the starch / PBAT composite material.

[0021] The present invention provides a method for preparing vinyl acetate grafted starch, comprising the following steps: mixing starch with water for gelatinization to obtain gelatinized starch; mixing the gelatinized starch, vinyl acetate and an initiator for grafting modification to obtain the vinyl acetate grafted starch. The present invention uses starch as a raw material, water as a solvent, and vinyl acetate as a grafting monomer to prepare grafted starch under the action of an initiator. Using the vinyl acetate grafted starch prepared by the present invention as a compatibilizer to compatibilize the starch / PBAT system can significantly improve the compatibility of starch and PBAT, and achieve complete compatibility between starch and PBAT; and the vinyl acetate grafted starch prepared by the present invention is low in price and fully biodegradable compared to other compatibilizers, making the starch / PBAT composite material one step closer to full starch plastics, and is expected to enter the field of food packaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is an electron microscope image of the original corn starch in Example 1;

[0023] Figure 2 This is an electron microscope image of the vinyl acetate grafted starch in Example 1;

[0024] Figure 3 The thermogravimetric curves of native corn starch and vinyl acetate grafted starch in Example 1;

[0025] Figure 4 The cross-sectional electron micrographs of starch / PBAT composite materials with different compatibilizers added to Example 2 and Comparative Examples 1 to 4 are shown in FIG. Figure 4 In the figure, a to e correspond to Comparative Example 1 (without a compatibilizer), Comparative Example 2 (TBC), Comparative Example 3 (TPPI), Comparative Example 4 (PVE), and Example 2 (vinyl acetate grafted starch) respectively. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing vinyl acetate grafted starch, comprising the following steps:

[0027] The starch is mixed with water for gelatinization to obtain gelatinized starch;

[0028] The gelatinized starch, vinyl acetate and an initiator are mixed for grafting modification to obtain the vinyl acetate grafted starch.

[0029] The present invention mixes starch with water for gelatinization to obtain gelatinized starch. The present invention has no special requirements for the starch, and starch well known to those skilled in the art can be used. In the present invention, the water is preferably distilled water; the gelatinization temperature is preferably 80-120°C, more preferably 95°C, the gelatinization temperature is preferably achieved in the form of a water bath, and the gelatinization time is preferably more than 30 minutes, subject to complete gelatinization. The present invention preferably adds water to the starch to prepare an emulsion with a solid content of 33wt%, and then heats the emulsion to 80-120°C for gelatinization; the gelatinization is preferably carried out under continuous stirring.

[0030] After obtaining gelatinized starch, the present invention mixes the gelatinized starch, vinyl acetate and an initiator for grafting modification to obtain the vinyl acetate grafted starch. In the present invention, the mass ratio of the starch to the vinyl acetate is preferably (0.8-1.2): (1.8-2.2), more preferably 1:2; the initiator is preferably ammonium cerium nitrate, the mass of the initiator is preferably 2.5-3.5% of the mass of the starch, more preferably 3%, and the addition of the initiator can improve the grafting rate and efficiency.

[0031] In the present invention, the specific operation of the graft modification preferably includes the following steps:

[0032] adding part of vinyl acetate and part of initiator to the gelatinized starch in sequence, and then simultaneously adding the remaining vinyl acetate and the remaining initiator dropwise to the obtained mixture;

[0033] The part of vinyl acetate is 1 / 3 of the total mass of vinyl acetate, and the part of initiator is 1 / 3 of the total mass of initiator; the dropping speed of the remaining vinyl acetate is 3s / drop, and the dropping speed of the remaining initiator is 20s / drop.

[0034] In the present invention, the temperature of the grafting modification is preferably 40 to 60°C, more preferably 50°C, and the time is preferably 3 to 5 hours. The time of the grafting modification is calculated from the time when the addition of the part of vinyl acetate is completed (the time of grafting modification does not include the time when vinyl acetate and the initiator are added). In an embodiment of the present invention, the time of the grafting modification is preferably 4 hours. Specifically, after adding the part of vinyl acetate, after stirring for 10 minutes, the part of the initiator is added and reacted for 50 minutes; then the remaining vinyl acetate and the remaining initiator are added dropwise at the same time, and the reaction is continued for 3 hours after the addition is completed. Because vinyl acetate is volatile, the above-mentioned mixing method adopted in the present invention is conducive to the full participation of vinyl acetate in the reaction.

[0035] In the present invention, the grafting modification is preferably carried out in a nitrogen atmosphere, and a condenser is used to condense and recover the volatile liquid throughout the process.

[0036] After the grafting modification, the present invention preferably cools the obtained reaction material to room temperature and then performs alcohol precipitation, and then filters to obtain the vinyl acetate grafted starch. In the present invention, the alcohol reagent used in the alcohol precipitation is preferably ethanol.

[0037] The present invention provides a vinyl acetate grafted starch prepared by the preparation method described in the above technical solution. The vinyl acetate grafted starch provided by the present invention is obtained by modifying native starch and is homologous to native starch, so it has a good volume expansion effect, and the vinyl acetate grafted starch is completely biodegradable, has no pollution to the environment, and is inexpensive.

[0038] The present invention provides the use of the vinyl acetate grafted starch described in the above technical solution as a compatibilizer in the preparation of a starch / PBAT composite material. Using the vinyl acetate grafted starch provided by the present invention as a compatibilizer to increase the compatibility of the starch / PBAT system can significantly improve the compatibility of starch and PBAT, and achieve complete compatibility of starch and PBAT; and the vinyl acetate grafted starch provided by the present invention can be completely degraded, so that the starch / PBAT composite material is one step closer to full starch plastic, and is expected to enter the field of food packaging.

[0039] The present invention provides a starch / PBAT composite material, comprising the following raw materials in parts by weight: 1 part of starch, 0.25-0.5 parts of glycerol, 0.3-0.6 parts of a compatibilizer, and 0.8-1.2 parts of PBAT (polybutylene terephthalate-adipate); the compatibilizer is the vinyl acetate grafted starch described in the above technical solution. In the present invention, the glycerol is preferably 0.4 parts, the compatibilizer is preferably 0.4 parts, and the PBAT is preferably 1 part.

[0040] In the present invention, the glycerol is used as a plasticizer to plasticize starch.

[0041] The starch / PBAT composite material provided by the present invention is completely compatible with starch and PBAT, and is a uniform starch-based bioplastic system. The starch / PBAT composite material has excellent mechanical properties, and the tensile strength can reach 28.6±1.5 MPa.

[0042] The present invention provides a method for preparing the starch / PBAT composite material described in the above technical solution, comprising the following steps:

[0043] The starch, glycerol and a compatibilizer are mixed and pre-plasticized, and the obtained mixture is subjected to twin-screw extrusion processing with PBAT to obtain the starch / PBAT composite material.

[0044] In the present invention, the pre-plasticization is preferably carried out in a high-speed mixer, and the pre-plasticization time is preferably more than 8 minutes. The present invention fully mixes starch, glycerol and a compatibilizer through the pre-plasticization to achieve a uniform dispersion effect, which is convenient for the next step of operation.

[0045] In the present invention, the twin-screw extruder used in the twin-screw extrusion process is preferably provided with six temperature zones from zone 1 to zone 6, with the temperatures being 140°C, 155°C, 150°C, 140°C, 140°C, and 140°C respectively, and the rotation speed of the twin-screw machine is preferably 280r / min.

[0046] In order to further illustrate the present invention, the vinyl acetate grafted starch and its preparation method and application and the starch / PBAT composite material and its preparation method provided by the present invention are described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.

[0047] Example 1

[0048] Vinyl acetate grafted starch, the preparation method is as follows:

[0049] 30 g corn starch was added to distilled water to prepare an emulsion with a solid content of 33 wt%, and then introduced into a 500 mL five-necked flask, heated to 95° C. in a water bath and stirred continuously to gelatinize the starch to obtain gelatinized starch;

[0050] The gelatinized starch was cooled to 50°C, nitrogen was filled for protection throughout the process, and volatile liquid was recovered by condensation of the condenser throughout the process. Some vinyl acetate was added (the total amount of vinyl acetate added was 60g, and 1 / 3 was added first). After stirring for 10 minutes, some initiator ammonium cerium nitrate was added (the total amount of ammonium cerium nitrate added was 3% of the total mass of starch, and 1 / 3 was added first, and ammonium cerium nitrate was pre-dissolved in distilled water). The reaction was continued for 50 minutes, and then the remaining 2 / 3 of vinyl acetate was added at a rate of 3s / drop using a constant pressure dropping funnel, and the remaining 2 / 3 of ammonium cerium nitrate was added at a rate of 20s / drop using a constant pressure dropping funnel (ensuring that vinyl acetate dripped before ammonium cerium nitrate), and the reaction was continued for 3 hours after all dripped (i.e., the total reaction time was 4 hours). After the reaction was completed, it was cooled to room temperature, ethanol was used for precipitation, and the filter was filtered and separated by a suction filter. The filtrate was taken out and its water content was measured and stored for use.

[0051] Example 2

[0052] A starch / PBAT composite material, using the vinyl acetate grafted starch prepared in Example 1 as a compatibilizer, the raw material dosage: 1 part by mass of starch, 0.4 part by mass of glycerol, 0.4 part by mass of vinyl acetate grafted starch, 1 part by mass of PBAT, the preparation method is as follows:

[0053] Starch, glycerol and vinyl acetate grafted starch are mixed in a mass ratio, pre-plasticized by a high mixer, and then PBAT is added and processed by a twin-screw extruder (the twin-screw extruder is provided with six temperature zones, and the temperatures are 140°C, 155°C, 150°C, 140°C, 140°C, and 140°C, respectively, and the speed of the twin-screw machine is 280r / min). After granulation, standard injection molded parts are processed by an injection molding machine.

[0054] Comparative Example 1

[0055] The vinyl acetate grafted starch was omitted, and the rest was the same as in Example 2.

[0056] Comparative Example 2

[0057] The vinyl acetate grafted starch in Example 2 was replaced by TBC (tributyl citrate), and the rest was the same as Example 2.

[0058] Comparative Example 3

[0059] The vinyl acetate grafted starch in Example 2 was replaced by TPPI (triphenyl phosphite), and the rest was the same as Example 2.

[0060] Comparative Example 4

[0061] The vinyl acetate grafted starch in Example 2 was replaced by PVE (soluble polyester, provided by Hubei Dingxin Environmental Protection Biomass Materials Co., Ltd.), and the rest was the same as Example 2.

[0062] Figure 1 and Figure 2 The electron microscope images of the original corn starch and the vinyl acetate grafted starch in Example 1 are shown in sequence. Figure 1 and Figure 2 It can be seen that before any modification, the appearance of starch is smooth. After esterification and grafting, the small starch particles become irregular and the damage to the particle surface becomes more serious because the vinyl acetate molecules can enter the starch molecules.

[0063] Figure 3The thermogravimetric curves of the original corn starch and the vinyl acetate grafted starch in Example 1. The weight loss process of the vinyl acetate grafted starch is divided into two stages. The first stage is mainly because the temperature destroys the combination of starch and water molecules. The weight loss temperature of the vinyl acetate grafted starch in this stage is about 120°C, and the mass loss is 11.09%. The mass of the starch remains basically unchanged when the temperature is 130-253°C; the second stage is the main stage of starch weight loss. At this time, the starch is decomposed by heat and the mass drops sharply. The mass loss at this time is due to the destruction of the starch molecular structure and the mass loss caused by the influence of air ashing. This stage can be regarded as a method for judging the thermal stability of the sample. At this stage, the mass of the vinyl acetate grafted starch loses 75.48%, and the initial temperature during the thermal decomposition process is about 260°C, and the mass loss is fastest at 314.9°C.

[0064] Figure 4 The cross-sectional electron micrographs of starch / PBAT composite materials with different compatibilizers added to Example 2 and Comparative Examples 1 to 4 are shown in FIG. Figure 4 In the figure, a to e correspond to Comparative Example 1 (without a compatibilizer), Comparative Example 2 (TBC), Comparative Example 3 (TPPI), Comparative Example 4 (PVE), and Example 2 (vinyl acetate grafted starch) in turn. By observing the electron microscope images of the composite materials with the addition of TBC and TPPI, it can be seen that there is a clear boundary between the gelatinized starch and PBAT, and there are gaps between the gelatinized starch and PBAT, and there are many pits on the PBAT matrix. This is because the adhesion between the starch and PBAT interface is poor, and when the starch is broken, the gelatinized starch particles fall off from the PBAT matrix; there are also many holes on the material with the addition of TPPI, and the gelatinized starch has agglomerated. Compared with the electron microscope images without the addition of a compatibilizer, the gelatinized starch agglomeration phenomenon is more serious and the gaps are more, which shows that TBC and TPPI do not compatibilize the two-phase system of gelatinized starch and PBAT, but have the opposite effect. Observing the electron microscope image of the composite material with PVE added, it can be seen that gelatinized starch and PBAT are melted together, and the boundary between them is almost invisible. Only a small amount of starch particles can be seen, and there is no obvious large particle and particle agglomeration phenomenon. This is because PVE plays the role of starch plasticizer, weakening the hydrogen bonding between starch molecules and within the molecule. At the same time, PVE plays the role of dispersant and lubricant in the composite material system, making the gelatinized starch particles dispersed more evenly, indicating that PVE can effectively increase the volume of gelatinized starch and PBAT. Observing the electron microscope image of the composite material with vinyl acetate grafted starch added, it can be seen that vinyl acetate grafted starch is used as a compatibilizer, and no starch particles are found on the entire interface. The entire interface is very evenly distributed with brittle hills, proving that the original starch and grafted starch are fully integrated with PBAT, have good compatibility, and form a uniform system.

[0065] According to ISO 527-2 standard, the tensile strength test was performed on the starch / PBAT composite materials of Example 2 and Comparative Examples 1 to 4 to which different compatibilizers were added. The test results are shown in Table 1:

[0066] Table 1 Tensile strength of starch / PBAT composite materials of Example 2 and Comparative Examples 1 to 4

[0067]

[0068]

[0069] It can be seen from Table 1 that the starch / PBAT composite material obtained by using vinyl acetate grafted starch as a compatibilizer in the present invention has excellent mechanical properties.

[0070] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A starch / PBAT composite material, characterized in that: The preparation method comprises the following raw materials in parts by weight: 1 part of starch, 0.4 part of glycerol, 0.4 part of a compatibilizer, and 1 part of PBAT; the compatibilizer is vinyl acetate grafted starch; The preparation method of the vinyl acetate grafted starch comprises the following steps: Adding water to starch to prepare an emulsion with a solid content of 33 wt%, and then heating the emulsion to 80-120° C. for gelatinization to obtain gelatinized starch; The gelatinized starch, vinyl acetate and an initiator are mixed for grafting modification to obtain the vinyl acetate grafted starch; the mass ratio of the starch to the vinyl acetate is 1:2, the initiator is ammonium cerium nitrate, and the mass of the initiator is 3% of the mass of the starch; The specific operation of the graft modification comprises the following steps: adding part of vinyl acetate and part of initiator to the gelatinized starch in sequence, and then simultaneously adding the remaining vinyl acetate and the remaining initiator dropwise to the obtained mixture; The part of vinyl acetate is 1 / 3 of the total mass of vinyl acetate, and the part of initiator is 1 / 3 of the total mass of initiator; the dropping speed of the remaining vinyl acetate is 3s / drop, and the dropping speed of the remaining initiator is 20s / drop; The temperature of the grafting modification is 40-60° C., and the time is 3-5 hours. The time of the grafting modification is calculated from the time when the addition of the part of the vinyl acetate is completed. The grafting modification is carried out in a nitrogen atmosphere.

2. The method for preparing the starch / PBAT composite material according to claim 1, characterized in that: The following steps are involved: The starch, glycerol and a compatibilizer are mixed and pre-plasticized, and the obtained mixture is subjected to twin-screw extrusion processing with PBAT to obtain the starch / PBAT composite material.

Citation Information

Patent Citations

  • Degradable starch-based plastic

    CN102690488A

  • Starch graft modification method, graft-modified starch and application of graft-modified starch in degradable plastics

    CN105524219A

  • Biodegradable materials from starch-grafted polymers

    US20050171249A1