Inorganic sulfide solid electrolyte and preparation method thereof
By introducing sodium and M elements into the sulfide solid electrolyte to form crystalline phase C and controlling the process parameters, the problem of sulfide electrolyte being sensitive to humid air is solved, and a sulfide solid electrolyte with high stability and high conductivity is achieved. Meet the needs of all-solid-state lithium secondary batteries.
Patent Information
- Application Number
- CN202311022071.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-08-14
AI Technical Summary
The existing sulfide solid electrolytes are sensitive to humid air and are prone to decomposition to produce toxic gases, resulting in a decrease in ionic conductivity, limiting their application in all-solid lithium secondary batteries.
By introducing sodium and M elements, the crystalline phase C is formed, the wet air stability of the sulfide solid electrolyte is improved, and the stability and conductivity of the material are ensured through appropriate process parameters such as CuKα ray diffraction peak position and heat treatment conditions. .
It significantly improves the wet air stability and ion conductivity of sulfide solid electrolytes, meets the use requirements of all-solid state batteries, simplifies production processes and reduces costs.
Smart Images

Figure CN117117299B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an inorganic sulfide solid electrolyte and a preparation method thereof. Background Art
[0002] Lithium-ion secondary batteries play an extremely important role in modern society, especially the development of new energy vehicles and large-scale energy storage, which has pushed them to an unprecedented height. With the continuous improvement of the energy density and safety requirements of power batteries, the existing liquid lithium-ion battery system has approached the upper limit of energy density, and the flammable organic electrolyte makes the safety hazards of high-energy liquid lithium-ion batteries more prominent. All-solid-state batteries that use non-flammable inorganic solid materials as electrolytes can not only eliminate the safety hazards caused by organic electrolyte leakage and thermal runaway inside the battery during use, but also can be used under extreme conditions such as high and low temperatures. The use of lithium metal negative electrodes will also further improve the energy density of all-solid-state lithium secondary batteries. Solid electrolytes are the most critical materials in all-solid-state batteries. The development of inorganic solid electrolytes with high stability and high lithium ion conductivity is the key to the development of high-performance all-solid-state batteries.
[0003] Among many solid electrolyte materials, sulfide solid electrolytes are currently the most studied and have the greatest application potential. The main reason is that sulfide electrolytes have ion conductivity comparable to that of liquid electrolytes. However, sulfide solid electrolytes are sensitive to water and decompose to produce toxic H2S gas when in contact with water, which reduces the ion conductivity. Therefore, the use conditions of sulfide solid electrolytes are very harsh and are not conducive to large-scale application. Therefore, it is necessary to develop a sulfide electrolyte material that is stable to wet air to meet the needs of practical application. Summary of the invention
[0004] In order to solve the above technical problems of the present invention, the present invention provides an inorganic sulfide solid electrolyte and a preparation method thereof. The present invention has found that by introducing sodium and M elements, a crystalline phase C can be formed in the main crystalline phase of the sulfide solid electrolyte. The crystalline phase C can greatly improve the wet air stability of the sulfide solid electrolyte.
[0005] According to a first aspect of the present invention, the present invention provides an inorganic sulfide solid electrolyte.
[0006] Containing Li and / or Na elements;
[0007] Containing P and / or halogen elements;
[0008] The crystal phase C is contained. The crystal phase C has a diffraction peak with an intensity of I at a position of 2θ=23.0±1.0° in powder X-ray diffraction using CuKα rays.
[0009] In the above scheme, an inorganic sulfide solid electrolyte contains Li and / or Na elements, P and / or halogen elements and crystalline phase C, wherein the crystalline phase C can greatly improve the wet air stability of the sulfide solid electrolyte. Through the synergistic effect of the above elements and the crystalline phase C, the obtained inorganic sulfide solid electrolyte has high ion conductivity and good air stability, which can further realize the use of sulfide solid electrolyte materials in dry rooms and meet the use requirements of all-solid-state batteries.
[0010] In one possible design, the crystal phase C has a diffraction peak at 2θ=23.0±0.5° in X-ray diffraction measurement using CuKα.
[0011] In the above scheme, the formation position of the diffraction peak of the crystalline phase C is further limited, which can better improve the wet air stability of the sulfide solid electrolyte.
[0012] In a possible design, in powder X-ray diffraction using CuK α rays, there are diffraction peaks at 2θ=25.5±0.5°, 29.9±0.5°, and 31.0±0.5°, and the diffraction peak intensities are I1, I2, and I3, respectively, and 0.020≤I / I1≤0.045, 0.025≤I / I2≤0.055, and 0.030≤I / I3≤0.060.
[0013] In the above aspect, when the inorganic sulfide solid electrolyte has the above diffraction peak, an ion conduction path is ensured in the crystal structure, and the ion conductivity is improved.
[0014] In one possible design, it is composed of the following general formula I:
[0015] Li 7+k-i-m Na i P j M k S l X m (I);
[0016] Wherein, M is one or more of Sn, 5i, Al, and Ge, X is one or more of F, Cl, Br, and I, 0.0<i≤0.5, 0.0≤k≤0.3, 3.0<l≤6.5, 0.0≤m<1.8, and i+k>0.
[0017] In the above scheme, the present invention has found that by introducing Na element and one or more elements of Sn, Si, Al, Ge, and Zr into the sulfide solid electrolyte, combined with adjusting the ratio of Li, Na, and M elements, a sulfide solid electrolyte containing a crystalline phase C can be obtained, and the electrolyte has higher wet air stability.
[0018] In one possible design, 0.0<i≤0.2, 0.00%<i / (7+kim)≤3.70%, 0.0≤k≤0.15, 4.5<l≤6.0, 0.0≤m<1.8, i+k>0.
[0019] In the above scheme, by further adjusting the ratio between the components in the inorganic sulfide solid electrolyte, a sulfide solid electrolyte containing a crystalline phase C can be better obtained, and the wet air stability of the inorganic sulfide solid electrolyte can be further improved.
[0020] In one possible design, 2.5≤k+j+1-i≤7.0; preferably, 5.0≤k+j+li≤7.0.
[0021] In the above scheme, by further limiting the ratio relationship between the components in the inorganic sulfide solid electrolyte, a sulfide solid electrolyte containing a crystalline phase C can be better obtained, and the wet air stability of the inorganic sulfide solid electrolyte can be further improved.
[0022] According to a second aspect of the present invention, the present invention also provides a method for preparing the above-mentioned inorganic sulfide solid electrolyte, comprising the following steps:
[0023] Step (1): under the protection of an inert atmosphere, the required raw materials are mixed according to a proportion and then ground;
[0024] Step (2): heat-treating the ground material under the protection of an inert atmosphere.
[0025] The preparation method of the inorganic sulfide solid electrolyte in the above scheme is to first mix the required raw materials according to the ratio under the protection of an inert atmosphere and then grind them to achieve a suitable fineness value, and mix the raw materials fully, which is conducive to obtaining a solid electrolyte with a crystalline phase C after subsequent heat treatment, and then heat treat the ground material under the protection of an inert atmosphere to remove volatile substances and moisture in the raw materials, improve the density and mechanical strength of the raw materials, improve the ion conductivity of the raw materials, and at the same time improve the chemical stability of the materials.
[0026] In a possible design, in step (1), the grinding is carried out in a ball mill, the grinding linear speed v is 7.5-16.0 m / s, the grinding time t is 3-24 h, and 5.0E+05m≤v×t≤6.5E+05m.
[0027] In the above scheme, by controlling the values of linear velocity v, time t and v×t during the grinding process within a reasonable range, it is beneficial to improve the stability and conductivity of the final inorganic sulfide solid electrolyte. If it is not processed under the above conditions, the stability of the material cannot be guaranteed.
[0028] In a possible design, in step (2), the heat treatment temperature T is 400°C-600°C, and the heat treatment time is 20h-48h.
[0029] In the above scheme, by controlling the temperature and time values during the heat treatment process within a reasonable range, it is beneficial to improve the stability and conductivity of the final inorganic sulfide solid electrolyte. If it is not treated under the above conditions, the stability of the material cannot be guaranteed.
[0030] According to the third aspect of the present invention, the present invention also provides a lithium secondary battery, comprising a positive electrode layer, a negative electrode layer and a solid electrolyte layer, wherein the solid electrolyte layer contains the above-mentioned inorganic sulfide solid electrolyte or the inorganic sulfide solid electrolyte prepared by the above-mentioned preparation method.
[0031] The technical solution provided by the present invention has the following beneficial effects:
[0032] The inorganic sulfide solid electrolyte of the present invention can obtain a sulfide solid electrolyte material containing a crystalline phase C by introducing an appropriate proportion of Na and M into the inorganic material and controlling the synthesis process parameters. The crystalline phase C can greatly improve the wet air stability of the sulfide solid electrolyte material. The sulfide solid electrolyte material can be further used in a drying room, simplifying the production process of solid-state batteries and reducing production costs. The sulfide solid electrolyte has high ion conductivity and good air stability, meeting the use requirements of all-solid-state batteries.
[0033] The inorganic sulfide solid electrolyte of the present invention is a twin-phase sulfide solid electrolyte, which is helpful for further understanding the chemical stability of the electrolyte in theoretical research and can obtain various types of high-stability electrolyte materials in practical application.
[0034] The preparation method of the inorganic sulfide solid electrolyte of the present invention is simple and effective, with low production cost. At the same time, the obtained solid electrolyte has good stability and high lithium ion conductivity, and is expected to solve the practical application problem of inorganic sulfide electrolyte as a high-performance all-solid-state lithium secondary battery electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 X-ray diffraction patterns of the solid electrolyte materials obtained in Comparative Example 4 and Example 4;
[0037] Figure 2 The EIS curves of the solid electrolyte material obtained in Comparative Example 4 before and after exposure;
[0038] Figure 3 This is the EIS curve of the solid electrolyte material obtained in Example 4 before and after exposure. DETAILED DESCRIPTION
[0039] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the art or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0040] In a glove box, weigh Li2S, Na2S, P2S5, LiCl, and MS2 according to the element ratios of the comparative examples and embodiments in Table 1, place the above raw materials in a 50ml zirconium oxide ball mill, and add 50g of 5mm diameter zirconium oxide balls. Place the sealed ball mill on the ball mill, and set the grinding speed and time according to the requirements in Table 1. Collect the ball-milled samples and seal them in a vacuum quartz tube for calcination. The calcination temperature is controlled by program temperature rise, and the temperature is raised from room temperature to the target temperature at a rate of 3°C / min, and kept warm for 20h to 48h. After sintering, cool it to 50°C to obtain the target solid electrolyte.
[0041] Solid electrolyte air stability test
[0042] The solid electrolyte materials obtained in Comparative Examples 1 to 7 and Examples 1 to 16 were subjected to air stability tests. In a glove box, 300 mg of the solid electrolyte material was weighed and placed in a 5 ml open glass bottle. The glass bottle was then placed in a reaction box with a specific humidity air flow and allowed to stand at room temperature for 24 hours. The relative humidity of the dry air was 10% and the air flow rate was 100 ml / min. After the standing period, the sample was taken out for ion conductivity testing and stability data was calculated.
[0043] Figure 1 The X-ray diffraction diagrams of the solid electrolyte materials obtained in Comparative Example 4 and Example 4 show that the main diffraction peaks of the solid electrolytes in Comparative Example 4 and Example 4 are sharp, which proves that the crystallinity of the solid electrolytes is good. The difference between the two is that Example 4 has an obvious diffraction peak at 23.1°, while Comparative Example 4 does not.
[0044] Figure 2The EIS curves of the solid electrolyte material obtained in Comparative Example 4 before and after exposure are shown in Figure 4. Based on the EIS curves, the ion conductivities before and after exposure are calculated to be 6.43 mS / cm and 4.61 mS / cm, respectively. The stability is calculated to be 4.61 / 6.43=71.7%.
[0045] Figure 3 The EIS curves of the solid electrolyte material obtained in Example 4 before and after exposure are shown in Figure 4. Based on the EIS curves, the ion conductivities before and after exposure are calculated to be 7.01 mS / cm and 6.28 mS / cm, respectively. The stability is calculated to be 6.28 / 7.01=89.6%.
[0046] Table 1 Composition, preparation conditions and performance data of Comparative Examples 1 to 7 and Examples 1 to 16
[0047]
[0048]
[0049] Table 1 summarizes the composition, preparation conditions and performance data of comparative examples 1 to 7 and examples 1 to 16. It can be seen from the experimental results of examples 1 to 16 in Table 1 that the inorganic sulfide solid electrolyte material provided by the present invention has high ion conductivity and good air stability, among which the inorganic sulfide solid electrolyte material obtained under the conditions of example 4 has the best air stability.
[0050] It can be seen from the experimental comparison results of Examples 1-16 and Comparative Examples 1-3 that by introducing Na and one or more elements of Sn, Si, Al, Ge, and Zr into the sulfide solid electrolyte, combined with the proportion adjustment of Li, Na, and M elements, a sulfide solid electrolyte containing a crystalline phase C can be obtained, and the electrolyte has higher wet air stability. It can be seen from the experimental results of Example 4 and Comparative Examples 4-5 that in the preparation process of the inorganic sulfide solid electrolyte, controlling the value of v×t within a reasonable range is conducive to the improvement of the ion conductivity and air stability of the material. It can be seen from the experimental comparison results of Example 4 and Comparative Examples 6-7 that in the preparation process of the inorganic sulfide solid electrolyte, controlling the heat treatment temperature T in step (2) within a reasonable range can significantly improve the ion conductivity and air stability of the material.
[0051] The inorganic sulfide solid electrolyte material provided by the present invention has a simple composition, readily available raw materials, a simple preparation method, and a low production cost. It also has good air stability and high lithium ion conductivity, and is expected to solve the practical application problem of inorganic sulfide electrolytes as high-performance all-solid-state lithium secondary battery electrolytes.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An inorganic sulfide solid electrolyte, characterized in that: Its composition is as follows: Li 7+k-i-m So i Q j M k S l X m (I); Wherein, M is one or more of Sn, Si, Al, Ge, X is one or more of F, Cl, Br, I, 0.0 <i≤0.5,0.0≤k≤0.3,3.0<l≤6.5,0.0≤m<1.8,i+k> 0; Contains a crystalline phase C, which has a diffraction peak at 2θ=23.0±1.0° and an intensity of I in powder X-ray diffraction using CuKα radiation; In powder X-ray diffraction using CuKα rays, there are diffraction peaks at 2θ=25.5±0.5°, 29.9±0.5°, and 31.0±0.5°, and the diffraction peak intensities are I1, I2, and I3, respectively, and 0.020≤I / I1≤0.045, 0.025≤I / I2≤0.055, and 0.030≤I / I3≤0.060; The preparation method of the inorganic sulfide solid electrolyte comprises the following steps: Step (1): under the protection of an inert atmosphere, the required raw materials are mixed according to a proportion and then ground; Step (2): heat treating the ground material under an inert atmosphere; the heat treatment temperature T is 400° C.-600° C.; In step (1), the grinding is carried out in a ball mill, the grinding linear velocity v is 7.5-16.0 m / s, the grinding time t is 3-24 h, and 5.0E+05m≤v×t≤6.5E+05m.
2. The inorganic sulfide solid electrolyte according to claim 1, characterized in that 0.0 <i≤0.2,0.00%<i / (7+k-i-m)≤3.70%,0.0≤k≤0.15,4.5<l≤6.0,0.0≤m<1.8,i+k> 0.
3. The inorganic sulfide solid electrolyte according to claim 2, characterized in that 2.5≤k+j+li≤7.
0.
4. The inorganic sulfide solid electrolyte according to claim 3, characterized in that 5.0≤k+j+li≤7.
0.
5. The inorganic sulfide solid electrolyte according to claim 1, characterized in that In step (2), the heat treatment time is 20h-48h.
6. A lithium secondary battery, characterized in that: The invention comprises a positive electrode layer, a negative electrode layer and a solid electrolyte layer, wherein the solid electrolyte layer contains the inorganic sulfide solid electrolyte according to any one of claims 1 to 5.