Antistatic nylon 66 composite masterbatch and preparation method thereof

By using the hydrogen bond and chemical bond coupling of modified carbon nanotubes to nylon resin in nylon 66 materials, the problems of uneven dispersion of conductive agents and insufficient antistatic properties are solved, and uniform conductivity and long-lasting antistatic properties are achieved. Electrostatic nylon 66 composite masterbatch.

CN117126433BActive Publication Date: 2024-11-19HUBEI YTS GRP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310908984.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-24
Publication Date
2024-11-19
Estimated Expiration
2043-07-24

AI Technical Summary

Technical Problem

The existing nylon 66 materials do not have anti-static properties, the conductive agent is unevenly dispersed and the anti-static properties are not long-lasting, mainly due to the poor dispersion and poor binding properties of carbon nanotubes.

Method used

By mixing the buffer, water, catechol and diethylene triamine, carbon nanotube modifier, fully react with multi-wall carbon nanotubes and mixing them with nylon resin emulsion, hydrogen bond coupling and chemical bonding are used to ensure carbon The nanotubes are evenly dispersed in nylon resin to avoid precipitation, achieving uniform conductivity and long-lasting anti-static properties.

Benefits of technology

It achieves uniformity of conductive properties and durability of antistatic properties, and is suitable for engineering plastic accessories that require antistatic properties, improving the electrostatic properties of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117126433B_ABST
    Figure CN117126433B_ABST
Patent Text Reader

Abstract

A method for preparing an antistatic nylon 66 composite masterbatch comprises the following steps: firstly mixing a carbon nanotube modifier and a multi-walled carbon nanotube in a desired proportion, obtaining modified carbon nanotubes after sufficient reaction, and then mixing the modified carbon nanotubes and a nylon resin emulsion in a desired proportion to obtain an antistatic nylon composite material, wherein the carbon nanotube modifier is prepared by mixing a buffer, water, catechol, and diethylenetriamine in a desired proportion. This design not only allows the modified carbon nanotubes to be uniformly dispersed in the nylon resin emulsion, thereby ensuring uniformity of conductive properties, but also prevents the modified carbon nanotubes from precipitating, and has a long-lasting antistatic property. When in use, the prepared antistatic nylon 66 composite masterbatch is added to the nylon resin as a reinforcing masterbatch for extrusion or injection molding into the required engineering plastic accessories, which is convenient to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer composite materials, and particularly relates to an antistatic nylon 66 composite masterbatch and a preparation method thereof. Background Art

[0002] The common nylon 66 material on the market is not conductive and does not have anti-static properties. It cannot be used in some occasions where the working voltage is high and anti-static properties are required. Conductive agents are usually added to the PA66 raw materials to achieve anti-static effects. However, there are defects such as uneven conductivity and short-lasting anti-static properties, which are mainly caused by uneven dispersion of the conductive agent and continuous precipitation of the conductive agent.

[0003] Chinese Patent: The invention patent with application number 202210377382.4 discloses a thermally conductive and insulating epoxy resin composite material, a preparation method and an application thereof. The method aims to solve the problem of poor compatibility between thermally conductive fillers and epoxy resins. First, boron nitride nanosheets (m-BNNSs) grafted with silane coupling agents and carbon nanotubes (DETA-MWCNTs) grafted with diethylenetriamine are ultrasonically dispersed in acetone, and then epoxy resin is added and heated and stirred until the acetone is completely evaporated. Finally, a curing agent and an accelerator are added, and the mixture is evenly stirred and then cured to obtain a thermally conductive and insulating epoxy resin. Lipid composite materials, on the one hand, this design uses diethylenetriamine DETA modification to wet the surface of MWCNTs, making them more dispersed in the epoxy resin, thereby reducing the microcapacitance caused by agglomeration, and on the other hand, D-MWCNTs and m-BNNSs can form a three-dimensional thermal conductive network in the epoxy resin matrix. Heat is rapidly transferred through the three-dimensional thermal conductive network, greatly improving the thermal conduction efficiency. Although this design can greatly improve the insulation performance, there are still problems such as poor dispersion of carbon nanotubes, uneven conductivity, weak bonding between carbon nanotubes and the matrix, and short-lasting antistatic performance. Summary of the invention

[0004] The purpose of the present invention is to provide an antistatic nylon 66 composite masterbatch with uniform conductive properties and durable antistatic properties and a preparation method thereof in view of the above-mentioned problems existing in the prior art.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows:

[0006] A method for preparing an antistatic nylon 66 composite masterbatch, the preparation method is carried out in the following steps:

[0007] S1, mixing a buffer, water, catechol, and diethylenetriamine in a desired proportion to prepare a carbon nanotube modifier;

[0008] S2, mixing the carbon nanotube modifier and the multi-walled carbon nanotubes in a desired ratio, and preparing the modified carbon nanotubes after sufficient reaction;

[0009] S3, mixing the modified carbon nanotubes and the nylon resin emulsion in a desired proportion to obtain an antistatic nylon 66 composite masterbatch.

[0010] In step S1, the buffer is tris(hydroxymethyl)aminomethane, and the mass ratio of the buffer, water, catechol and diethylenetriamine is 10-15:100-120:5-10:5-10.

[0011] In step S3, the mass ratio of the modified carbon nanotubes to the nylon resin emulsion is 2-4:20-30.

[0012] In step S3, the nylon resin emulsion is prepared by mixing the nylon resin and the solvent in a desired proportion, heating until the nylon resin is completely dissolved, and obtaining the nylon resin emulsion, wherein the mass ratio of the nylon resin to formic acid is 10-20:40-50.

[0013] In step S3, after adding the modified carbon nanotubes into the nylon resin emulsion in a required proportion, stirring at 75-85° C. until the solvent is completely volatilized, an antistatic nylon 66 composite masterbatch is obtained.

[0014] In step S3, the nylon resin is nylon 66 resin, and the solvent is formic acid.

[0015] In step S2, the mass ratio of the carbon nanotube modifier to the multi-walled carbon nanotube is 40-50:2-4.

[0016] In step S2, after the carbon nanotube modifier and multi-walled carbon nanotubes are mixed in the required proportion, the mixed system is first placed at 45-55° C. for ultrasonic vibration for at least 2 hours, and then the mixed system is diluted with deionized water and fully washed, and the deionized water is removed by drying to obtain modified carbon nanotubes.

[0017] The multi-walled carbon nanotube has an outer diameter of 30-50 nm, a length of 10-20 μm, and a purity of more than 95%.

[0018] An antistatic nylon 66 composite masterbatch is prepared by the above-mentioned preparation method.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The invention discloses a method for preparing an antistatic nylon 66 composite masterbatch, comprising the steps of firstly mixing a carbon nanotube modifier and a multi-walled carbon nanotube in a required proportion, and obtaining modified carbon nanotubes after sufficient reaction, and then mixing the modified carbon nanotubes and a nylon resin emulsion in a required proportion to obtain an antistatic nylon 66 composite masterbatch, wherein the carbon nanotube modifier is prepared by mixing a buffer, water, catechol, and diethylenetriamine in a required proportion, firstly reacting catechol with diethylenetriamine to generate a catechol-polyamine polymer, and the catechol-polyamine polymer can react with The carbon nanotubes are coupled by hydrogen bonds, and after coupling, the carbon nanotubes are dispersed in the nylon resin emulsion, and no agglomeration occurs during dispersion, thereby ensuring uniformity of conductive performance. The catechol-polyamine polymer can also be chemically bonded with the PA66 macromolecular chain, thereby generating a strong coupling force with the nylon resin substrate, avoiding precipitation of the carbon nanotubes, and having a long-lasting antistatic performance. When used, the antistatic nylon 66 composite masterbatch prepared by the preparation method is added to the nylon resin as a reinforcing masterbatch for extrusion or injection molding into the required engineering plastic accessories, which is convenient to use. Therefore, the present invention not only ensures uniformity of conductive performance, but also has good long-lasting antistatic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the structure of the modified carbon nanotubes in the present invention.

[0022] Figure 2 It is a schematic structural diagram of the antistatic nylon 66 composite masterbatch in the present invention. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with specific implementations and drawings.

[0024] A method for preparing an antistatic nylon 66 composite masterbatch, the preparation method is carried out in the following steps:

[0025] S1, mixing a buffer, water, catechol, and diethylenetriamine in a desired proportion to prepare a carbon nanotube modifier;

[0026] S2, mixing the carbon nanotube modifier and the multi-walled carbon nanotubes in a desired ratio, and preparing the modified carbon nanotubes after sufficient reaction;

[0027] S3, mixing the modified carbon nanotubes and the nylon resin emulsion in a desired proportion to obtain an antistatic nylon 66 composite masterbatch.

[0028] In step S1, the buffer is tris(hydroxymethyl)aminomethane, and the mass ratio of the buffer, water, catechol and diethylenetriamine is 10-15:100-120:5-10:5-10.

[0029] In step S3, the mass ratio of the modified carbon nanotubes to the nylon resin emulsion is 2-4:20-30.

[0030] In step S3, the nylon resin emulsion is prepared by mixing the nylon resin and the solvent in a desired proportion, heating until the nylon resin is completely dissolved, and obtaining the nylon resin emulsion, wherein the mass ratio of the nylon resin to formic acid is 10-20:40-50.

[0031] In step S3, after adding the modified carbon nanotubes into the nylon resin emulsion in a required proportion, stirring at 75-85° C. until the solvent is completely volatilized, an antistatic nylon 66 composite masterbatch is obtained.

[0032] In step S3, the nylon resin is nylon 66 resin, and the solvent is formic acid.

[0033] In step S2, the mass ratio of the carbon nanotube modifier to the multi-walled carbon nanotube is 40-50:2-4.

[0034] In step S2, after the carbon nanotube modifier and multi-walled carbon nanotubes are mixed in the required proportion, the mixed system is first placed at 45-55° C. for ultrasonic vibration for at least 2 hours, and then the mixed system is diluted with deionized water and fully washed, and the deionized water is removed by drying to obtain modified carbon nanotubes.

[0035] The multi-walled carbon nanotube has an outer diameter of 30-50 nm, a length of 10-20 μm, and a purity of more than 95%.

[0036] An antistatic nylon 66 composite masterbatch is prepared by the above-mentioned preparation method.

[0037] The principle of the present invention is described as follows:

[0038] First, catechol and diethylenetriamine undergo polymerization reaction in a tris(hydroxymethyl)aminomethane buffer to generate a catechol-polyamine polymer containing multiple reactive groups. The catechol-polyamine polymer has the following three structures:

[0039] The first one:

[0040]

[0041] Second type:

[0042]

[0043] The third type:

[0044]

[0045] The three structures of the catechol-polyamine polymer exist simultaneously and can be converted into each other, which is a dynamic equilibrium. The catechol-polyamine polymer has a strong reactivity and can be coupled with the multi-walled carbon nanotubes through hydrogen bonds after mixing with the multi-walled carbon nanotubes (one of the reaction processes is shown in Figure 1 ), after coupling, the multi-walled carbon nanotubes will not agglomerate when dispersed in the nylon resin emulsion, and finally the modified carbon nanotubes are mixed with the nylon resin emulsion, and the catechol-polyamine polymer can also be chemically bonded with the nylon resin macromolecule chain, specifically, the benzene ring is directly coupled with the nylon macromolecule chain, and the oxygen in the carbonyl and hydroxyl groups is coupled with the nylon macromolecule chain (for the specific reaction process, see Figure 2 ), thereby generating a strong coupling force with the nylon resin substrate and preventing the carbon nanotubes from precipitating.

[0046] Embodiment 1:

[0047] A method for preparing an antistatic nylon 66 composite masterbatch is specifically carried out according to the following steps:

[0048] S1, mixing a buffer, water, catechol, and diethylenetriamine in a desired proportion, stirring and dissolving them at room temperature to prepare a carbon nanotube modifier, wherein the buffer is trishydroxymethylaminomethane, and the addition amounts of the buffer, distilled water, catechol, and diethylenetriamine are 10Kg, 100Kg, 5Kg, and 5Kg, respectively;

[0049] S2, mixing the carbon nanotube modifier and the multi-walled carbon nanotubes in the required proportion, stirring and dissolving the mixture, placing the mixture under ultrasonic vibration at 50°C for 2h, then diluting the mixture with deionized water and washing it thoroughly, drying and removing the deionized water, to obtain modified carbon nanotubes, wherein the addition amounts of the carbon nanotube modifier and the multi-walled carbon nanotubes are 40Kg and 2Kg respectively;

[0050] The modified carbon nanotubes and nylon resin emulsion are added in an amount of 2 kg and 20 kg, respectively. The nylon resin emulsion is prepared by mixing nylon resin and solvent in a desired proportion, heating to 80°C and stirring for 10 minutes until the nylon resin is completely dissolved, to obtain the nylon resin emulsion. The nylon resin and formic acid are added in an amount of 10 kg and 40 kg, respectively. The nylon resin is nylon 66 resin, the solvent is formic acid, and the multi-walled carbon nanotubes are selected to have an outer diameter of 30-50 nm, a length of 10-20 μm, and a purity of >95%.

[0051] S3. Mix the modified carbon nanotubes and nylon resin emulsion in the required proportion, stir at 80° C. until the formic acid is completely volatilized, and then dry at a constant temperature of 80° C. until the weight no longer decreases, thereby obtaining the antistatic 66 composite masterbatch.

[0052] Embodiment 2:

[0053] The difference from Example 1 is that:

[0054] In step S1, the added amounts of the buffer, distilled water, catechol, and diethylenetriamine are 15Kg, 120Kg, 10Kg, and 10Kg, respectively;

[0055] In step S2, the added amounts of the carbon nanotube modifier and multi-walled carbon nanotubes are 50Kg and 4Kg respectively; the added amounts of the modified carbon nanotubes and nylon resin emulsion are 4Kg and 30Kg respectively; the added amounts of the nylon resin and formic acid are 20Kg and 50Kg respectively.

[0056] Embodiment 3:

[0057] The difference from Example 1 is that:

[0058] In step S1, the added amounts of the buffer, distilled water, catechol, and diethylenetriamine are 13Kg, 110Kg, 8Kg, and 8Kg, respectively;

[0059] In step S2, the added amounts of the carbon nanotube modifier and multi-walled carbon nanotubes are 45Kg and 3Kg respectively; the added amounts of the modified carbon nanotubes and nylon resin emulsion are 3Kg and 25Kg respectively; the added amounts of the nylon resin and formic acid are 15Kg and 45Kg respectively.

[0060] Performance Test:

[0061] In order to verify the high conductivity of the antistatic 66 composite masterbatch prepared by the method of the present invention, the antistatic 66 composite masterbatch prepared in Example 1 was used as a reinforcing masterbatch and mixed with a PA66 substrate for extrusion granulation to obtain a material as a test example, wherein the mass percentage of the reinforcing masterbatch was 5%, and the PA66 substrate without adding the reinforcing masterbatch was used as a comparative example, and the following performance tests were performed respectively:

[0062] Table 1 Performance test results

[0063] project Comparative Example Test Case <![CDATA[Axial tensile strength / MPa > 52 83.5 <![CDATA[Tensile modulus of elasticity / GPa > 1.11 1.62 <![CDATA[Impact strength / KJ / m 3 > 6.5 35.2 <![CDATA[Wear rate (V) (300 °C) / (10 -7 cm 3 N·m)]]> 0.50 0.36 Glass transition temperature / ℃ 58-62 90-95 Water absorption / % 1-2 0.2-0.5 Volume resistivity / Ω·cm <![CDATA[2.6×10 13 ]]> <![CDATA[9.8×10 2 ]]>

[0064] As can be seen from Table 1, the volume resistivity of the test example is much lower than that of the comparative example. This is because a large amount of modified carbon nanotubes are evenly dispersed in the PA66 substrate, and the carbon nanotubes have high conductivity, so that the prepared reinforced masterbatch has high conductivity, that is, antistatic performance; it can be seen that the use of the antistatic nylon 66 composite masterbatch prepared by the present invention as a reinforced masterbatch can significantly improve the electrostatic performance, and is suitable for electronic devices, electrical products, high-precision instruments and meters, automotive engineering plastic parts, household appliances and other places where current breakdown and anti-static are required to be avoided, and it plays the role of anti-static, conductive, and working voltage resistance.

Claims

1. A method for preparing an antistatic nylon 66 composite masterbatch, characterized in that: The preparation method is carried out in the following steps: S1, mixing a buffer, water, catechol, and diethylenetriamine in a desired proportion to prepare a carbon nanotube modifier; S2, mixing the carbon nanotube modifier and the multi-walled carbon nanotubes in a desired ratio, and preparing the modified carbon nanotubes after sufficient reaction; In step S2, after the carbon nanotube modifier and the multi-walled carbon nanotubes are mixed in the required proportion, the mixed system is placed at 45-55° C. for ultrasonic vibration for at least 2 hours, and then the mixed system is diluted with deionized water and fully washed, and the deionized water is removed by drying to obtain modified carbon nanotubes; S3, mixing the modified carbon nanotubes and the nylon resin emulsion in a desired proportion to obtain an antistatic nylon 66 composite masterbatch; In step S3, after adding the modified carbon nanotubes into the nylon resin emulsion in a required proportion, stirring at 75-85° C. until the solvent is completely volatilized, an antistatic nylon 66 composite masterbatch is obtained.

2. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 1, characterized in that: In step S1, the buffer is tris(hydroxymethyl)aminomethane, and the mass ratio of the buffer, water, catechol and diethylenetriamine is 10-15:100-120:5-10:5-10.

3. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 1 or 2, characterized in that: In step S3, the mass ratio of the modified carbon nanotubes to the nylon resin emulsion is 2-4:20-30.

4. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 1 or 2, characterized in that: In step S3, the nylon resin emulsion is prepared by mixing the nylon resin and the solvent in a desired proportion, heating until the nylon resin is completely dissolved, and obtaining the nylon resin emulsion, wherein the mass ratio of the nylon resin to formic acid is 10-20:40-50.

5. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 4, characterized in that: In step S3, the nylon resin is nylon 66 resin, and the solvent is formic acid.

6. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 1 or 2, characterized in that: In step S2, the mass ratio of the carbon nanotube modifier to the multi-walled carbon nanotube is 40-50:2-4.

7. The method for preparing an antistatic nylon 66 composite masterbatch according to claim 1 or 2, characterized in that: The multi-walled carbon nanotubes have an outer diameter of 30-50 nm, a length of 10-20 μm, and a purity of more than 95%. 8.An antistatic nylon 66 composite masterbatch, characterized by: The antistatic nylon 66 composite masterbatch is prepared by the preparation method described in claim 1.