A welding method for C44300 tin brass
Through the tungsten argon arc welding method combined with the use of silver welding wire and argon gas protection, the problems caused by zinc oxidation evaporation and thermal conductivity in C44300 tin brass welding are solved, and the welding quality and post-weld performance are improved.
Patent Information
- Application Number
- CN202311155143.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-09-08
AI Technical Summary
C44300 tin brass produces smoke due to zinc oxidation and evaporation during the welding process, which affects the welding quality. Its good thermal conductivity leads to rapid cooling of the welding pool, the generation of pores and thermal cracks, weld reinforcement and lack of penetration, which affects mechanics. Performance and appearance shaped.
Using the tungsten arc welding method, first use BCu91PAg silver welding wire to form the base layer, and then use BAg50CuZn silver welding wire to form the cover layer. Control the welding temperature below 50°C, and grind the groove and clean it with acetone before welding. Use high-quality Pure argon gas protects the welding pool, and the weld reinforcement is controlled by a copper rod.
It effectively reduces zinc evaporation, prevents the generation of pores and thermal cracks, and ensures the mechanical properties and corrosion resistance of welded joints. The appearance after welding is beautiful, the deformation is small, and the tensile strength is not less than 310MPa.
Smart Images

Figure CN117161517B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tin brass welding, and in particular to a welding method for C44300 tin brass. Background Art
[0002] Tin brass with the grade of HSn72-1 (codenamed C44300) is an important material for manufacturing copper alloy seamless tubes for heat exchangers and condensers in thermal power generation, ships and vessels, offshore petroleum, mechanical chemical industry and other industrial sectors.
[0003] At present, the copper alloy seamless pipe made of C44300 tin brass has the following problems during welding:
[0004] (1) Since the tin brass of C44300 contains a large amount of zinc, and the boiling point of zinc is only 907℃, the zinc element is easily oxidized and evaporated due to high temperature during welding, generating white smoke, which not only hinders the welder's observation and operation of the molten pool, but also leads to the decrease of mechanical properties and corrosion resistance of the welded joint;
[0005] (2) During welding, external impurities and air easily enter the welding pool, producing cuprous oxide (chemical formula: Cu2O) and welding gas. Since the thermal conductivity of C44300 tin brass is good, the cooling speed of the welding pool is fast, so that the gas in the welding pool has no time to float up, resulting in the formation of weld pores; and since the solubility of cuprous oxide in the welding pool is much higher than that of solidified copper and low-melting-point eutectic, it is easy to cause welding thermal cracks;
[0006] (3) The weld height inside the pipe is too high during welding, affecting product quality;
[0007] (4) Due to the high thermal conductivity of C44300 tin brass and the difficulty in melting the C44300 tin brass base metal, the weld metal and the base metal cannot be well fused, and incomplete penetration is prone to occur;
[0008] (5) Since the tin brass of C44300 is relatively soft, the deformation after welding is more serious and the appearance is poor.
[0009] Therefore, how to find a welding method for C44300 tin brass with high welding efficiency, which can effectively reduce zinc evaporation and burning to ensure the mechanical properties, mechanical properties and corrosion resistance of the welded joint, as well as beautiful appearance and small deformation after welding has always been a technical problem that technicians in this field have been trying to solve. Summary of the invention
[0010] The invention aims to provide a welding method for C44300 tin brass with beautiful appearance after welding, small deformation and good performance after welding.
[0011] To achieve the above object, the present invention adopts the following technical solution: a welding method of C44300 tin brass, comprising the following steps:
[0012] Step (1): processing a groove on the end of the C44300 tin brass base material to be welded, and grinding and cleaning the groove;
[0013] Step (2): assembling the grooves of the ends of the pipes to be welded of two C44300 tin brass base materials opposite to each other, with the gap between the grooves of the ends of the pipes to be welded being 2 to 3 mm, and introducing high-purity argon gas into the two C44300 tin brass base materials;
[0014] Step (3): Use tungsten inert gas welding to weld the groove joints of the two C44300 tin brass base materials into which high-purity argon gas has been introduced. The specific tungsten inert gas welding steps are as follows:
[0015] Step (3.1): firstly, use a silver welding wire with a grade of BCu91PAg to weld the groove joint of two C44300 tin brass base materials, stop welding after each welding for 1 minute, wait until the temperature of the C44300 tin brass base material drops to 50°C, and then continue welding for 1 minute until a circle is welded at the groove joint of the two C44300 tin brass base materials to form a base layer; wherein, the welding current is 90-120A, the welding voltage is 11-15V, the welding speed is 7-10cm / min, and the flow rate of helium is 13-18L / min;
[0016] Step (3.2): After the temperature of the base layer drops to room temperature, a silver welding wire with a grade of BAg50CuZn is used to weld the groove joints of two C44300 tin brass base materials on the base layer, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material drops to 50°C, the welding is continued for 1 minute until a circle is welded on the base layer to form a cover layer, thereby obtaining a C44300 tin brass base material welding product; wherein the welding current is 100-130A, the welding voltage is 13-17V, the welding speed is 10-12cm / min, and the flow rate of helium is 13-18L / min.
[0017] Furthermore, in the aforementioned C44300 tin brass welding method, in which: in step (3.1), the welding current is 100 A, the welding voltage is 13 V, the welding speed is 8 cm / min, and the helium flow rate is 15 L / min.
[0018] Furthermore, in the aforementioned C44300 tin brass welding method, in which: in step (3.2), the welding current is 120A, the welding voltage is 15V, the welding speed is 11cm / min, and the helium flow rate is 15L / min.
[0019] Furthermore, in the aforementioned C44300 tin brass welding method, in which: in step (1), the groove of the pipe end to be welded of the C44300 tin brass base material is cleaned with acetone.
[0020] Furthermore, the aforementioned C44300 tin brass welding method, wherein: in step (2), it also includes a copper rod, the outer diameter of the copper rod is adapted to the inner diameter of the C44300 tin brass mother material so that the copper rod can be adapted to be inserted into the C44300 tin brass mother material, and a circle of limiting grooves with a groove depth of 2 mm is provided on the outer peripheral wall of the end of the copper rod, and the copper rod is inserted into one of the C44300 tin brass mother materials, and the copper rod is moved inward until its limiting groove is opposite to the groove joint of the two C44300 tin brass mother materials.
[0021] Through the implementation of the above technical solution, the beneficial effects of the present invention are:
[0022] (1) Before welding, the welding groove should be polished and cleaned with acetone to effectively reduce impurities and avoid unnecessary impurity reactions that cause weld porosity;
[0023] (2) Use low current and short welding time during welding to avoid the pipe being at high temperature for a long time, effectively reduce the evaporation and burning of zinc, which not only facilitates the welder's observation and operation of the welding pool, but also ensures the mechanical properties and corrosion resistance of the welded joint;
[0024] (3) Since the silver-containing silver welding wire has very good fluidity, in order to prevent welding nodules or excessive weld height inside the pipe, the copper rod is set to ensure that the weld height inside the pipe is no higher than 2mm, thereby ensuring product quality;
[0025] (4) When welding, first use silver welding wire with the grade of BCu91PAg to form the base layer, and then use silver welding wire with the grade of BAg50CuZn to form the cover layer. When welding, use the corresponding welding process and control the interlayer temperature below 50°C. This can make the weld metal and the C44300 tin brass base material fuse and penetrate well, which not only makes the appearance of the weld beautiful and the deformation small, but also ensures the mechanical properties and corrosion resistance of the welded joint;
[0026] (6) During welding, high-purity argon gas is used to protect the inside of the tube and the welding pool, reducing the chance of external impurities and air entering the welding pool, reducing the generation of cuprous oxide and welding gas in the welding pool, and thus reducing the generation of welding thermal cracks and weld porosity;
[0027] (7) The tensile strength and bending strength of the welded C44300 tin brass base material are high, and the tensile strength is not less than 310MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention provides a method for welding C44300 tin brass, and a schematic diagram of the relative position relationship between a C44300 tin brass base material and a copper rod during welding.
[0029] Figure 2 This is a schematic diagram of the structure of the copper rod.
[0030] Figure 3 This is a schematic diagram of the product appearance of a C44300 tin brass base material welded product after welding using a C44300 tin brass welding method described in a third specific embodiment of the present invention.
[0031] Figure 4 This is a schematic diagram of the appearance of the inner wall weld of a C44300 tin brass base material welded product after welding using a C44300 tin brass welding method as described in the third specific embodiment of the present invention.
[0032] Figure 5 This is a test report of a C44300 tin brass base material welding product after welding using a C44300 tin brass welding method as described in the third specific embodiment of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Specific embodiment 1
[0034] like Figure 1 , Figure 2 As shown, the welding method of C44300 tin brass comprises the following steps:
[0035] Step (1): processing a groove 2 on the end of the pipe to be welded of the C44300 tin brass base material 1, and grinding and cleaning the groove 2; wherein the groove 2 of the end of the pipe to be welded of the C44300 tin brass base material 1 is cleaned with acetone;
[0036] Step (2): assembling the grooves 2 of the ends of the pipes to be welded of two C44300 tin brass base materials 1, with the gap h between the grooves of the ends of the pipes to be welded being 2 mm, and introducing high-purity argon gas into the two C44300 tin brass base materials 1;
[0037] A copper rod 3 is prepared, the outer diameter of the copper rod 3 is adapted to the inner diameter of the C44300 tin brass mother material 1, so that the copper rod 3 can be inserted into the C44300 tin brass mother material 1, and a limiting groove 4 with a groove depth of 2 mm is provided on the outer peripheral wall of the end of the copper rod 3, and then the copper rod 3 is inserted into one of the C44300 tin brass mother materials 1, and the copper rod 3 is moved inward until its limiting groove 4 faces the groove joint 5 of the two C44300 tin brass mother materials;
[0038] Step (3): using tungsten inert gas argon welding to weld the groove joint 5 of the two C44300 tin brass base materials 1 into which high-purity argon gas has been introduced; the specific tungsten inert gas argon welding steps are as follows:
[0039] Step (3.1): firstly, a silver welding wire with a grade of BCu91PAg is used to weld the groove joint 5 of two C44300 tin brass base materials 1, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material 1 drops to 50°C, the welding is continued for 1 minute until a circle is welded at the groove joint 5 of the two C44300 tin brass base materials 1 to form a base layer; wherein, the welding current is 90A, the welding voltage is 11V, the welding speed is 7cm / min, and the flow rate of helium is 13L / min;
[0040] Step (3.2): After the temperature of the base layer drops to room temperature, a silver welding wire with a grade of BAg50CuZn is used to weld the groove joint 5 of the two C44300 tin brass base materials 1 on the base layer, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material drops to 50° C., the welding is continued for 1 minute until a circle is welded on the base layer to form a cover layer, thereby obtaining a C44300 tin brass base material welding product; wherein the welding current is 100A, the welding voltage is 13V, the welding speed is 10cm / min, and the flow rate of helium is 13L / min. Specific embodiment 2
[0041] like Figure 1 , Figure 2 As shown, the welding method of C44300 tin brass comprises the following steps:
[0042] Step (1): processing a groove 2 on the end of the pipe to be welded of the C44300 tin brass base material 1, and grinding and cleaning the groove 2; wherein the groove 2 of the end of the pipe to be welded of the C44300 tin brass base material 1 is cleaned with acetone;
[0043] Step (2): the grooves 2 of the pipe ends to be welded of two C44300 tin brass base materials 1 are connected and assembled, the gap h between the grooves of the pipe ends to be welded of the two C44300 tin brass base materials is 3 mm, and high-purity argon gas is introduced into the two C44300 tin brass base materials 1;
[0044] A copper rod 3 is prepared, the outer diameter of the copper rod 3 is adapted to the inner diameter of the C44300 tin brass mother material, so that the copper rod 3 can be inserted into the C44300 tin brass mother material 1, and a limiting groove 4 with a groove depth of 2 mm is provided on the outer peripheral wall of the end of the copper rod 3, and then the copper rod 3 is inserted into one of the C44300 tin brass mother materials 1, and the copper rod 3 is moved inward until its limiting groove 4 is opposite to the groove joint 5 of the two C44300 tin brass mother materials 1;
[0045] Step (3): using tungsten inert gas argon welding to weld the groove joint 5 of the two C44300 tin brass base materials 1 into which high-purity argon gas has been introduced; the specific tungsten inert gas argon welding steps are as follows:
[0046] Step (3.1): firstly, a silver welding wire with a grade of BCu91PAg is used to weld the groove joint 5 of two C44300 tin brass base materials 1, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material 1 drops to 50°C, the welding is continued for 1 minute until a circle is welded at the groove joint 5 of the two C44300 tin brass base materials 1 to form a base layer; wherein, the welding current is 120A, the welding voltage is 15V, the welding speed is 10cm / min, and the flow rate of helium is 18L / min;
[0047] Step (3.2): After the temperature of the base layer drops to room temperature, a silver welding wire with a grade of BAg50CuZn is used to weld the groove joint 5 of the two C44300 tin brass base materials 1 on the base layer, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material 1 drops to 50° C., the welding is continued for 1 minute until a circle is welded on the base layer to form a cover layer, thereby obtaining a C44300 tin brass base material welding product; wherein the welding current is 130A, the welding voltage is 17V, the welding speed is 12cm / min, and the flow rate of helium is 18L / min. Specific embodiment three
[0048] like Figure 1 , Figure 2 As shown, the welding method of C44300 tin brass comprises the following steps:
[0049] Step (1): processing a groove 2 on the end of the pipe to be welded of the C44300 tin brass base material 1, and grinding and cleaning the groove 2; wherein the groove 2 of the end of the pipe to be welded of the C44300 tin brass base material 1 is cleaned with acetone;
[0050] Step (2): assembling the grooves 2 of the ends of the pipes to be welded of two C44300 tin brass base materials 1, with the gap h between the grooves of the ends of the pipes to be welded being 2 mm, and introducing high-purity argon gas into the two C44300 tin brass base materials 1;
[0051] A copper rod 3 is prepared, the outer diameter of the copper rod 3 is adapted to the inner diameter of the C44300 tin brass mother material 1, so that the copper rod 3 can be inserted into the C44300 tin brass mother material 1, and a limit groove 4 with a groove depth of 2 mm is provided on the outer peripheral wall of the end of the copper rod 3, and then the copper rod 3 is inserted into one of the C44300 tin brass mother materials 1, and the copper rod 3 is moved inward until its limit groove 4 is opposite to the groove joint 5 of the two C44300 tin brass mother materials 1;
[0052] Step (3): using tungsten inert gas argon welding to weld the butt joint of the groove 2 of the two C44300 tin brass base materials 1 into which high-purity argon gas has been introduced; the specific tungsten inert gas argon welding steps are as follows:
[0053] Step (3.1): firstly, a silver welding wire with a grade of BCu91PAg is used to weld the groove joint 5 of two C44300 tin brass base materials 1, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material 1 drops to 50°C, the welding is continued for 1 minute until a circle is welded at the groove joint 5 of the two C44300 tin brass base materials 1 to form a base layer; wherein, the welding current is 100A, the welding voltage is 13V, the welding speed is 8cm / min, and the flow rate of helium is 15L / min;
[0054] Step (3.2): After the temperature of the base layer drops to room temperature, a silver welding wire with a grade of BAg50CuZn is used to weld the groove joint 5 of the two C44300 tin brass base materials 1 on the base layer, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material 1 drops to 50° C., the welding is continued for 1 minute until a circle is welded on the base layer to form a cover layer, thereby obtaining a C44300 tin brass base material welding product; wherein, the welding current is 120A, the welding voltage is 15V, the welding speed is 11cm / min, and the flow rate of helium is 15L / min.
[0055] The appearance of the obtained C44300 tin brass base material welding product is as follows Figure 3 As shown, the appearance of the inner wall weld of the C44300 tin brass base material welded product is as follows Figure 4 As shown;
[0056] In order to test the tensile strength and bending strength of the obtained C44300 tin brass base material welding product, the obtained C44300 tin brass base material welding product is divided into at least 6 segments along the axial direction, and 6 of the segments are taken and marked with corresponding sample numbers, namely: 02-1, 02-2, 02-3, 02-4, 02-5, 02-6, 02-1 and 02-2 are subjected to tensile tests, and 02-3, 02-4, 02-5, 02-6 are subjected to bending tests. The test results of each segment are shown in the figure. Figure 5 shown; from Figure 5 It can be known that the tensile strength of the C44300 tin brass base material welded product is not less than 310MPa.
[0057] The advantages of the present invention are:
[0058] (1) Before welding, the welding groove should be polished and cleaned with acetone to effectively reduce impurities and avoid unnecessary impurity reactions that cause weld porosity;
[0059] (2) Use low current and short welding time during welding to avoid the pipe being at high temperature for a long time, effectively reduce the evaporation and burning of zinc, which not only facilitates the welder's observation and operation of the welding pool, but also ensures the mechanical properties and corrosion resistance of the welded joint;
[0060] (3) Since the silver-containing silver welding wire has very good fluidity, in order to prevent welding nodules or excessive weld height inside the pipe, the copper rod is set to ensure that the weld height inside the pipe is no higher than 2mm, thereby ensuring product quality;
[0061] (4) When welding, first use silver welding wire with the grade of BCu91PAg to form the base layer, and then use silver welding wire with the grade of BAg50CuZn to form the cover layer. When welding, use the corresponding welding process and control the interlayer temperature below 50°C. This can make the weld metal and the C44300 tin brass base material fuse and penetrate well, which not only makes the appearance of the weld beautiful and the deformation small, but also ensures the mechanical properties and corrosion resistance of the welded joint;
[0062] (6) During welding, high-purity argon gas is used to protect the inside of the tube and the welding pool, reducing the chance of external impurities and air entering the welding pool, reducing the generation of cuprous oxide and welding gas in the welding pool, and thus reducing the generation of welding thermal cracks and weld porosity;
[0063] (7) The tensile strength and bending strength of the welded C44300 tin brass base material are high, and the tensile strength is not less than 310MPa.
[0064] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A welding method for C44300 tin brass, characterized in that: The following steps are involved: Step (1): processing a groove on the end of the C44300 tin brass base material to be welded, and grinding and cleaning the groove; Step (2): assembling the grooves of the ends of the pipes to be welded of two C44300 tin brass base materials opposite to each other, with the gap between the grooves of the ends of the pipes to be welded being 2 to 3 mm, and introducing high-purity argon gas into the two C44300 tin brass base materials; Step (3): Use tungsten inert gas welding to weld the groove joints of the two C44300 tin brass base materials into which high-purity argon gas has been introduced. The specific tungsten inert gas welding steps are as follows: Step (3.1): firstly, use a silver welding wire with a grade of BCu91PAg to weld the groove joint of two C44300 tin brass base materials, stop welding after each welding for 1 minute, wait until the temperature of the C44300 tin brass base material drops to 50°C, and then continue welding for 1 minute until a circle is welded at the groove joint of the two C44300 tin brass base materials to form a base layer; wherein, the welding current is 90-120A, the welding voltage is 11-15V, the welding speed is 7-10cm / min, and the flow rate of helium is 13-18L / min; Step (3.2): After the temperature of the base layer drops to room temperature, a silver welding wire with a grade of BAg50CuZn is used to weld the groove joints of two C44300 tin brass base materials on the base layer, and the welding is stopped after each welding for 1 minute. After the temperature of the C44300 tin brass base material drops to 50°C, the welding is continued for 1 minute until a circle is welded on the base layer to form a cover layer, thereby obtaining a C44300 tin brass base material welding product; wherein the welding current is 100-130A, the welding voltage is 13-17V, the welding speed is 10-12cm / min, and the flow rate of helium is 13-18L / min.
2. A method for welding C44300 tin brass according to claim 1, characterized in that: In step (3.1), the welding current is 100 A, the welding voltage is 13 V, the welding speed is 8 cm / min, and the helium flow rate is 15 L / min.
3. A method for welding C44300 tin brass according to claim 1, characterized in that: In step (3.2), the welding current is 120A, the welding voltage is 15V, the welding speed is 11cm / min, and the helium flow rate is 15L / min.
4. A method for welding C44300 tin brass according to claim 1, 2 or 3, characterized in that: In step (1), the groove of the pipe end to be welded of the C44300 tin brass base material is cleaned with acetone.
5. A method for welding C44300 tin brass according to claim 1, 2 or 3, characterized in that: In step (2), a copper rod is also included, the outer diameter of the copper rod is adapted to the inner diameter of the C44300 tin brass mother material, so that the copper rod can be adapted to be inserted into the C44300 tin brass mother material, and a limit groove with a groove depth of 2 mm is provided on the outer peripheral wall of the end of the copper rod. The copper rod is inserted into one of the C44300 tin brass mother materials, and the copper rod is moved inward until its limit groove faces the groove joint of the two C44300 tin brass mother materials.
Citation Information
Patent Citations
Welding process method of brass H62
CN102699496A
Welding method for large-specification HSn62-1 tin brass
CN113664341A
Heat transfer tube constructed of tin brass alloy
US20050247380A1