Metal laminated material with single gradient hierarchical porous structure and preparation method thereof
The metal laminated materials with single-gradient hierarchical porous structures are formed through diffusion welding additive manufacturing and dealloyment technology, which solves the problem of insufficient catalytic and mechanical properties of traditional porous materials, and achieves efficient catalytic and long-life effects.
Patent Information
- Application Number
- CN202311031971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-08-16
AI Technical Summary
The uniform pore size of traditional pore metal materials leads to insufficient catalytic performance, poor mechanical properties, and the service life cannot meet market demand.
Diffusion welding additive manufacturing technology is used to stack different metals together, and an infinite solid solution layer is formed by hot pressing. Combined with dealloyment technology, a metal laminated material with a single gradient hierarchical porous structure is formed.
It improves catalytic efficiency and mechanical properties, extends the service life of the material, and meets the needs of high mass transfer rates and high catalytic performance.
Smart Images

Figure CN117162594B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal catalytic materials, and in particular to a metal laminate material with a single gradient graded porous structure and a preparation method thereof. Background Art
[0002] Nano-metal porous materials are widely used in catalysis, medical and other fields due to their large specific surface area and high porosity. However, the pore size and ligament size of traditional porous materials are uniform, which cannot meet the actual process requirements of high mass transfer efficiency and high catalytic performance. Therefore, researchers turned to studying new porous materials. On the basis of traditional porous materials, they also gave their ligaments porous structures, so that smaller secondary pores appeared in nano-metal materials, hoping to use larger pores for flow exchange control, while smaller pores can expose more catalytically active positions, increase the required catalytic surface area, and ultimately improve catalytic performance.
[0003] The presence of secondary pores on the ligaments does increase the specific surface area of the material, thereby exposing more active sites and improving the catalytic performance to a certain extent. However, in the actual factory catalytic process, the surface tension of some organic waste liquid media is relatively large, and too small a pore size will lead to excessive actual surface tension, making it impossible for the small pores in the catalyst to contact the medium to be catalyzed, and thus the secondary pores cannot effectively play their role. On the other hand, due to the small structural size and large surface area of porous metals, slight changes in surface stress will lead to significant changes in the internal stress and strain of the material, resulting in poor mechanical properties; at the same time, due to the inheritance of crystal defects and dislocations in the precursor into the porous structure, traditional porous structure metal materials are very brittle, making the life and maintenance of metal porous materials unable to meet current market demand. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies of the prior art and provide a metal laminate material with a single gradient graded porous structure and a preparation method thereof. Dissimilar metals are stacked together through diffusion welding additive manufacturing technology, and diffused into each other through hot pressing treatment to form an infinite solid solution layer. The active metal atoms are then removed by dealloying to form a metal laminate material with a single gradient graded porous structure. The metal laminate material has a high mass transfer rate and catalytic efficiency, excellent mechanical properties and a long service life.
[0005] The first aspect of the present invention relates to a method for preparing a metal laminate material having a single gradient hierarchical porous structure, comprising the following steps:
[0006] S1. Cleaning the surfaces of the first metal and the second metal to remove processing oil and other impurities on the metal surfaces; wherein there are differences in chemical activity and thermodynamic stability between the first metal and the second metal, and it is defined that the first metal is more active than the second metal, and the diffusion rate of the first metal is faster than that of the second metal;
[0007] S2, after the first metal and the second metal cleaned in step S1 are sequentially stacked N times, a diffusion welding additive manufacturing process is used to eliminate the physical interface between the first metal and the second metal, so that the first metal and the second metal are tightly combined to obtain a first intermediate; wherein N≥1;
[0008] S3, heat-treating the first intermediate so that the first metal and the second metal diffuse into each other to form an infinite solid solution, thereby obtaining a second intermediate; wherein the second intermediate comprises a second metal layer and an infinite solid solution layer;
[0009] S4, subjecting the second intermediate to dealloying treatment to remove the first metal atoms in the infinite solid solution layer, thereby forming a porous structure and obtaining a metal laminate material;
[0010] Among them, in the porous structure, the pore size shows a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.
[0011] In an optional embodiment, the thickness X of the desired infinite solid solution layer is determined as follows:
[0012] W<X<2W;
[0013] Wherein, W is a relatively larger thickness value between the thickness of the first metal and the thickness of the second metal.
[0014] In an optional embodiment, the thickness Y of the first metal is 3 μm to 200 μm, and the thickness Z of the second metal is 3 μm to 200 μm.
[0015] In an alternative embodiment, the element species of the first metal and the second metal are two elements in the same group of elements.
[0016] In an optional embodiment, when N=1, in the porous structure, the pore size presents a single gradient change from small to large along the second metal layer toward one side.
[0017] In an optional embodiment, when N>1, in the porous structure, the pore size presents a single gradient change from small to large along the second metal layer toward both sides.
[0018] In an optional embodiment, the specific process of the diffusion welding additive manufacturing process is as follows:
[0019] The first metal and the second metal cleaned in step S1 are sequentially stacked on each other and placed in a vacuum hot pressing furnace, the pressure is applied to 5-20 MPa, and the temperature is controlled to T1, and the first heat preservation treatment is performed under the protection of nitrogen atmosphere until the physical interface between the first metal and the second metal is eliminated; wherein the control range of temperature T1 is 0.5T m ≤T1<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal.
[0020] In an optional embodiment, the heat treatment process is as follows:
[0021] The first intermediate is sealed with a vacuum quartz tube and protected by a nitrogen atmosphere, placed in a muffle furnace, and subjected to a second insulation treatment at a temperature of T2; wherein the temperature T2 is set according to the requirement that the atoms of the first metal and the second metal can break the physical interface and form an infinite solid solution layer; and the time of the second insulation treatment is set according to the required thickness X of the infinite solid solution layer.
[0022] In an optional embodiment, the control range of temperature T2 is 0.5T m ≤T2<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal.
[0023] In an optional embodiment, the time of the second heat preservation treatment is determined as follows:
[0024] According to formula (1), the time t of the second heat preservation treatment without heat loss is obtained:
[0025]
[0026] Where X is the thickness of the required infinite solid solution layer, m; X1 is the diffusion thickness of the first metal in the second metal, m; X2 is the diffusion thickness of the second metal in the first metal, m; t is the time of the second insulation treatment without heat loss, s; D1 is the diffusion coefficient of the first metal in the second metal, m 2 / s; D2 is the diffusion coefficient of the second metal in the first metal, m 2 / s;
[0027] Heat preservation is performed at time t to obtain an infinite solid solution layer with a thickness of X'. When X'<X, the time of the second heat preservation treatment is increased until the thickness of the infinite solid solution layer meets the requirements; when X'>X, the time of the second heat preservation treatment is reduced until the thickness of the infinite solid solution layer meets the requirements.
[0028] The second aspect of the present invention relates to a metal laminate material with a single gradient graded porous structure prepared by the aforementioned method. The metal laminate material has a porous structure, and the pore size in the porous structure presents a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.
[0029] Compared with the prior art, the present invention has the following significant beneficial effects:
[0030] The preparation method of the present invention uses diffusion welding additive manufacturing technology to stack dissimilar metals that can form an infinite solid solution together. The atoms at the interface of the two metals diffuse each other due to the concentration gradient, and the metal interface disappears due to atomic diffusion, and a bimetallic infinite solid solution layer appears. The atomic diffusion in the infinite solid solution layer presents a gradient distribution with dense density in the middle and dispersed on both sides. Then, combined with dealloying technology, the active metal atoms are dissolved to form a periodic porous structure. The pore size of each porous structure has a single gradient change from the middle to the sides, from the first channel to the second channel. The average pore size of the second channel is much larger than the average pore size of the first channel, and the first channel and the second channel form a graded porous structure.
[0031] In the metal laminate material with a single gradient graded porous structure of the present invention, the size difference between the inner first pores and the outer second pores is maintained within an appropriate range, so that the small-sized first pores can allow the catalytic medium to enter therein, so that the catalytic active sites in the small-sized holes can play a role, and the large-sized second pores maintain the mass transfer speed, thereby improving the mass transfer rate and catalytic efficiency in tandem.
[0032] The metal laminate material obtained by the method of the present invention contains a diffused metal layer, which is equivalent to introducing a reinforcement structure into the laminated porous structure, so that the metal laminate material has better mechanical properties than pure porous materials, solves the problem of poor mechanical properties of current metal porous materials, is more conducive to maintenance, and has a better service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the process mechanism of the method for preparing the metal laminate material with a single gradient graded porous structure of the present invention.
[0034] Figure 2 It is one of the schematic diagrams for the derivation of formula (1) of the present invention.
[0035] Figure 3 It is one of the schematic diagrams for the derivation of formula (1) of the present invention.
[0036] Figure 4 This is the OM diagram of the original stacking interface of Example 1 of the present invention.
[0037] Figure 5 1 is a SEM EDS mapping diagram of the CuAg stack thermal diffusion of Example 1 of the present invention; wherein a is a cross-sectional diagram of the CuAg stack thermal diffusion, and b, c, and d are all element distribution diagrams in a.
[0038] Figure 6 yes Figure 5 Energy spectrum line scan.
[0039] Figure 7 It is a morphology image of the cross section of the sample after the CuAg stack is heat-treated and chemically dealloyed in Example 1 of the present invention; wherein a is the overall morphology, and b, c, and d are morphology images at different high magnifications at different positions on a, respectively.
[0040] Figure 8 It is a morphology image of the sample surface after chemical dealloying of the CuAg stack after heat treatment in Example 1 of the present invention; wherein, a is the overall morphology, and b, c, and d are high-magnification morphology images at the same position on a, respectively.
[0041] Fig. 9 It is a morphology image of the cross section of the sample after chemical dealloying of the AlZn stack heat treatment of Example 2 of the present invention; wherein, a is the overall morphology, and b, c, and d are morphology images at different high magnifications at different positions on a, respectively. DETAILED DESCRIPTION
[0042] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.
[0043] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.
[0044] Combination Figure 1 As shown, in a preferred embodiment of the present invention, a method for preparing a metal laminate material having a single gradient graded porous structure is provided, comprising the following steps:
[0045] S1. Cleaning the surfaces of the first metal and the second metal to remove processing oil and other impurities on the metal surfaces; wherein there are differences in chemical activity and thermodynamic stability between the first metal and the second metal, and it is defined that the first metal is more active than the second metal, and the diffusion rate of the first metal is faster than that of the second metal;
[0046] S2, after the first metal and the second metal cleaned in step S1 are sequentially stacked N times, a diffusion welding additive manufacturing process is used to eliminate the physical interface between the first metal and the second metal, so that the first metal and the second metal are tightly combined to obtain a first intermediate; wherein N≥1;
[0047] S3, heat-treating the first intermediate so that the first metal and the second metal diffuse into each other to form an infinite solid solution, thereby obtaining a second intermediate; wherein the second intermediate comprises a second metal layer and an infinite solid solution layer;
[0048] S4, subjecting the second intermediate to dealloying treatment to remove the first metal in the infinite solid solution layer, thereby forming a porous structure and obtaining a metal laminate material;
[0049] Among them, in the porous structure, the pore size shows a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.
[0050] It is understandable that in the above method, the chemical activity of the first metal and the second metal is not limited. It only needs to satisfy that there is a difference between the two. There must be a situation where one of the metals is more active. For the convenience of description, it is defined that the first metal is more active than the second metal.
[0051] Similarly, as long as they are two different metals, they must have different thermodynamic stabilities, that is, different diffusion rates. Therefore, in the above method, the thermodynamic stability of the first metal and the second metal is not limited. For the sake of convenience of description, it is defined that the diffusion rate of the first metal is faster than that of the second metal.
[0052] In an optional embodiment, the thickness X of the desired infinite solid solution layer is taken as follows:
[0053] W<X<2W;
[0054] Wherein, W is a relatively larger thickness value between the thickness of the first metal and the thickness of the second metal.
[0055] The thickness of the infinite solid solution layer needs to be kept within a certain range. If the infinite solid solution layer is too thin, the first metal layer will exist in the formed second intermediate, and the first metal layer will be corroded during dealloying, resulting in the inability to link the porous structure of the final second metal element together, the material is broken, and the metal laminate material cannot be obtained;
[0056] If the infinite solid solution layer is too thick, it will affect the thickness of the inactive second metal layer, or even the second metal layer will not exist, thus affecting the mechanical properties of the laminated material.
[0057] In an optional embodiment, the thickness Y of the first metal is 3 μm to 200 μm, and the thickness Z of the second metal is 3 μm to 200 μm; the thicknesses of the first metal and the second metal are preferably equal, but it should be understood that the thicknesses of the first metal and the second metal may not be equal.
[0058] In an optional embodiment, the element types of the first metal and the second metal are two elements in the same group of elements, for example, Cu and Ag, Cu and Au, etc.
[0059] Metals of the same group of elements can diffuse into each other during heat treatment to form an infinite solid solution. It should be understood that the element types of the first metal and the second metal include but are not limited to elements of the same group, as long as the corresponding two elements can form an infinite solid solution; for example, Al and Zn, Al and Sn, do not belong to the same group of elements, but it can be seen from the phase diagram that the two elements can form an infinite solid solution.
[0060] In an optional embodiment, when N=1, in the porous structure, the pore size presents a single gradient change from small to large along the second metal layer toward one side.
[0061] In an optional embodiment, when N>1, that is, the first metal, the second metal, the first metal, the second metal are cyclically stacked in sequence, or the second metal, the first metal, the second metal, the first metal, the first metal are cyclically stacked in sequence, in the resulting porous structure, the pore size shows a single gradient change from small to large along the second metal layer to both sides.
[0062] A porous structure with a single gradient change from the first channel to the second channel formed on both sides along the second metal layer, and the second metal layer connected to the porous structure are defined as a first structure. In particular, in the case of multilayer superposition with N>2, the obtained metal laminate material contains multiple first structures, so that the structure of the metal laminate material is periodic.
[0063] In an optional embodiment, the pore size varies in a gradient, and the maximum average pore size is 5 to 20 times the minimum average pore size.
[0064] In an optional embodiment, the specific process of the diffusion welding additive manufacturing process is as follows:
[0065] The first metal and the second metal cleaned in step S1 are sequentially stacked on each other and placed in a vacuum hot pressing furnace, the pressure is applied to 5-20 MPa, and the temperature is controlled to T1, and the first heat preservation treatment is performed under the protection of nitrogen atmosphere until the physical interface between the first metal and the second metal is eliminated; wherein the control range of temperature T1 is 0.5T m ≤T1<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal.
[0066] It should be understood that the ultimate goal of additive manufacturing using diffusion welding is to diffuse and connect the superimposed first metal and the second metal so that the parts will not separate; it can be understood that the physical interface between the first metal and the second metal is eliminated and a tight bond is formed. At this time, mutual diffusion has occurred between the first metal and the second metal, thereby causing the physical interface between the first metal and the second metal to be eliminated and connected.
[0067] In an optional embodiment, the heat treatment process is as follows:
[0068] The first intermediate is sealed with a vacuum quartz tube and protected by a nitrogen atmosphere, placed in a muffle furnace, and subjected to a second insulation treatment at a temperature of T2; wherein the temperature T2 is set according to the requirement that the atoms of the first metal and the second metal can break the physical interface and form an infinite solid solution layer; and the time of the second insulation treatment is set according to the required thickness X of the infinite solid solution layer.
[0069] It can be understood that during the second heat preservation treatment, the pressure condition of 5 to 20 MPa can continue to be selected, or there is no need to further set the pressure condition.
[0070] In an optional embodiment, the control range of temperature T2 is 0.5T m ≤T2<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal.
[0071] In an optional embodiment, the time of the second heat preservation treatment is determined as follows:
[0072] According to formula (1), the time t of the second heat preservation treatment without heat loss is obtained:
[0073]
[0074] Where X is the thickness of the required infinite solid solution layer, m; X1 is the diffusion thickness of the first metal in the second metal, m; X2 is the diffusion thickness of the second metal in the first metal, m; t is the time of the second insulation treatment without heat loss, s; D1 is the diffusion coefficient of the first metal in the second metal, m 2 / s; D2 is the diffusion coefficient of the second metal in the first metal, m 2 / s;
[0075] Heat preservation is performed at time t to obtain an infinite solid solution layer with a thickness of X'. When X'<X, the time of the second heat preservation treatment is increased until the thickness of the infinite solid solution layer meets the requirements; when X'>X, the time of the second heat preservation treatment is reduced until the thickness of the infinite solid solution layer meets the requirements.
[0076] It is understandable that in the actual insulation process, heat will be lost. Therefore, the thickness of the infinite solid solution layer cannot reach the required thickness. According to formula (1), the reference insulation time can be obtained. By adjusting the insulation time, the infinite solid solution layer of the required thickness can be achieved through reasonable matching of the diffusion coefficient and control of the thermal diffusion time, realizing the alternating distribution structure of the elemental metal layer and the solid solution layer.
[0077] It should be understood that the time of the first insulation treatment can be obtained based on empirical values or calculated based on formula (1). Since the ultimate goal of additive manufacturing using diffusion welding is to diffuse and connect the superimposed first metal and second metal, the problem of heat loss does not need to be considered.
[0078] The derivation process of formula (1) is as follows:
[0079] Diffusion couple whose components at both ends are not affected by diffusion
[0080] The mass concentration is C A The metal A rod and the mass concentration is C B Metal B rods are welded together with the welding surface perpendicular to the X-axis, and then heated and kept warm for different times. The mass concentration near the welding surface (x=0) will change to varying degrees. It is assumed that the test rod is long enough to ensure that the original concentration is always maintained at both ends of the diffusion couple.
[0081] Therefore, the analytical expression of mass concentration C changing with distance x and time t is shown in equation (2):
[0082]
[0083] In the formula, C A is the mass concentration of metal A; C B is the mass concentration of metal B; x is the diffusion distance, m; t is the diffusion time, s; D is the diffusion coefficient, m 2 / s.
[0084] Based on formula (2), formula (1) is derived:
[0085] Combination Figure 2 As shown, the diffusion direction of the first metal to the second metal is defined as the positive direction; the position where the diffusion starts at the physical interface between the first metal and the second metal is defined as the origin (in an ideal state, the interface when the first metal just diffuses to the second metal, the position when the first metal atom breaks the physical interface); the point where the first metal diffusion stops is defined as the diffusion end point surface (in an ideal state, the interface when the first metal diffuses to the second metal ends, on the diffusion end point surface, all the metal atoms on the surface are second metal atoms), and the intersection with the coordinate axis is the diffusion end point; the distance between the origin and the diffusion end point is the diffusion thickness X1 of the first metal in the second metal;
[0086] therefore,
[0087] The concentration of the first metal at which diffusion starts at the physical interface between the first metal and the second metal is defined as the diffusion start concentration of the first metal, denoted as C1;
[0088] The concentration of the second metal at which diffusion starts at the physical interface between the first metal and the second metal is defined as the diffusion start concentration of the second metal, denoted as C2;
[0089] After the diffusion of the first metal to the second metal is completed, the concentration of the first metal at the diffusion end point surface is defined as the diffusion end concentration of the first metal, which is recorded as C3;
[0090] After the diffusion of the first metal to the second metal is completed, the concentration of the second metal at the diffusion end point surface is defined as the diffusion end concentration of the second metal, which is recorded as C4;
[0091] Wherein, the diffusion coefficient of the first metal is D1, and the diffusion coefficient of the second metal is D2;
[0092] Under ideal conditions, when diffusion begins, the first metal atom breaks the physical interface, that is, at the origin, C1 is 100% and C2 is 0 (C1=1, C2=0); when diffusion ends, the diffusion end point is all the second metal atoms, that is, at the end point, C3=0, C4=1; the physical meaning of the negative sign in the calculation result represents the diffusion direction.
[0093] Simplifying formula (2), the formula of the diffusion thickness X1 of the first metal in the second metal and the heat treatment time t is as follows:
[0094]
[0095] Combination Figure 3 As shown, the diffusion direction of the second metal to the first metal is defined as the positive direction (the positive direction defined at this time has no connection with the positive direction when deriving formula (3)); the position where the diffusion starts at the physical interface between the first metal and the second metal is defined as the origin (in an ideal state, the interface when the second metal just diffuses into the first metal, the position when the second metal atom breaks the physical interface); the point where the second metal diffusion stops is defined as the diffusion end point surface (in an ideal state, the interface when the second metal diffuses into the first metal ends, on the diffusion end point surface, all the metal atoms on the surface are first metal atoms), and the intersection with the coordinate axis is the diffusion end point; the distance between the origin and the diffusion end point is the diffusion thickness X2 of the second metal in the first metal;
[0096] therefore,
[0097] The concentration at which the second metal starts to diffuse at the physical interface between the first metal and the second metal is defined as the diffusion start concentration of the second metal, denoted as C5;
[0098] The concentration at which the second metal starts to diffuse at the physical interface between the first metal and the second metal is defined as the diffusion starting concentration of the first metal, denoted as C6;
[0099] After the second metal is diffused into the first metal, the second metal concentration at the diffusion end point surface is defined as the diffusion end concentration of the second metal, which is recorded as C7;
[0100] After the second metal diffuses into the first metal, the first metal concentration at the diffusion end point surface is defined as the diffusion end concentration of the first metal, which is recorded as C8;
[0101] Wherein, the diffusion coefficient of the first metal is D1, and the diffusion coefficient of the second metal is D2;
[0102] Under ideal conditions, when diffusion begins, the moment the second metal atom breaks the physical interface, that is, at the origin, C5 is 100% and C6 is 0 (C5=1, C6=0); when diffusion ends, the diffusion end point is all the first metal atoms, that is, at the end point, C7=0, C8=1; the physical meaning of the negative sign in the calculation result represents the diffusion direction.
[0103] Simplifying formula (2), the formula of the diffusion thickness X2 of the second metal in the first metal and the heat treatment time t is as follows:
[0104]
[0105] Based on equations (3) and (4), equation (1) is derived, and the required thickness X of the infinite solid solution layer is:
[0106]
[0107] Where X is the thickness of the required infinite solid solution layer, m; X1 is the diffusion thickness of the first metal in the second metal, m; X2 is the diffusion thickness of the second metal in the first metal, m; t is the holding time, s; D1 is the diffusion coefficient of the first metal in the second metal, m 2 / s; D2 is the diffusion coefficient of the second metal in the first metal, m 2 / s.
[0108] The temperature is kept at a holding time of t to obtain an infinite solid solution layer with a thickness of X'. Since the heat cannot be fully used for diffusion in the actual production process, there is a certain amount of heat loss. Therefore, the thickness of the infinite solid solution layer obtained at the holding time t is different from the expected value. It is necessary to adjust the holding time with reference to the obtained X'.
[0109] When X'<X, increase the holding time until the thickness of the infinite solid solution layer meets the requirement; when X'>X, reduce the holding time until the thickness of the infinite solid solution layer meets the requirement.
[0110] In an optional embodiment, a chemical dealloying method is used to remove relatively active metal atoms in the second intermediate; it is understandable that the chemical dealloying method is a prior art and is not further limited herein.
[0111] like Figure 1 As shown, in an exemplary embodiment of the present invention, a method for preparing a metal laminate material having a single gradient hierarchical porous structure is provided, comprising the following specific steps:
[0112] (1) Clean the surface impurities of metal A and metal B (purity: 99%, the thickness of the two metals is equal, 3 μm to 200 μm) and set aside.
[0113] (2) The two metal foils processed in step (1) are stacked in the order of ABAB... to the required number of layers, and the number of stacking times N ≥ 1, such as Figure 1 Part a of
[0114] Then put it into the vacuum hot pressing furnace mold, apply a pressure of 5MPa~20MPa in the vacuum hot pressing furnace, and control the temperature to T1. Perform the first heat preservation treatment under the protection of nitrogen atmosphere until the physical interface between metal A and metal B is eliminated and a connection is formed, that is, mutual diffusion begins between the two metals to form a diffusion layer, such as Figure 1 Part b of
[0115] Among them, the control range of T1 is 0.5T m ≤T1<T 软, when the melting point of metal A is greater than the melting point of metal B, T m is the melting point of metal B, T 软 is the softening temperature of metal B; when the melting point of metal A is lower than the melting point of metal B, T m is the melting point of metal A, T 软 is the softening temperature of metal A.
[0116] (3) passing the material treated in step (2) through a vacuum quartz sealing tube, using an argon atmosphere to protect it from high-temperature oxidation, and performing a second heat preservation treatment in a muffle furnace to form an infinite solid solution layer of a desired thickness between the two metals;
[0117] Among them, the control range of heat treatment temperature T2 is 0.5T m ≤T2<T 软 , when the melting point of metal A is greater than the melting point of metal B, T m is the melting point of metal B, T 软 is the softening temperature of metal B; when the melting point of metal A is lower than the melting point of metal B, T m is the melting point of metal A, T 软 is the softening temperature of metal A;
[0118] The time for the second insulation treatment is determined as follows:
[0119] According to formula (1), the time t of the second heat preservation treatment without heat loss is obtained:
[0120]
[0121] Where X is the thickness of the required infinite solid solution layer, m; X1 is the diffusion thickness of the first metal in the second metal, m; X2 is the diffusion thickness of the second metal in the first metal, m; t is the time of the second insulation treatment without heat loss, s; D1 is the diffusion coefficient of the first metal in the second metal, m 2 / s; D2 is the diffusion coefficient of the second metal in the first metal, m 2 / s;
[0122] Heat preservation is performed at time t to obtain an infinite solid solution layer with a thickness of X'. When X'<X, the time of the second heat preservation treatment is increased until the thickness of the infinite solid solution layer meets the requirements; when X'>X, the time of the second heat preservation treatment is reduced until the thickness of the infinite solid solution layer meets the requirements.
[0123] During the heat treatment process, the concentration gradient of the two metal atoms at the interface changes due to the thermal diffusion. The metal interface disappears due to atomic diffusion, and a double metal diffusion layer appears. In this diffusion layer, the number of metal A atoms gradually decreases in the direction of metal A diffusing to metal B; similarly, the number of metal B atoms gradually decreases in the direction of metal B diffusing to metal A. Therefore, the diffusion layer is subject to Fick's law, making the atomic diffusion present a gradient distribution with dense in the middle and dispersed on both sides, such as Figure 1 Part c.
[0124] (4) placing the material treated in step (3) into a dealloying solution for chemical dealloying in a constant temperature water bath to remove the metal A component with more active chemical properties and obtain a porous B material.
[0125] Through dealloying technology, active metal atoms are dissolved, such as Figure 1 The d part reduces the dissolution of A atoms and forms pores. Due to the influence of diffusion, the pores close to the pure metal layer B are small, and the pores far away from the pure metal layer B are large, forming a single gradient porous structure. The pore size of each porous structure has a gradient change from small to large from the middle to both sides, thus forming a single gradient graded porous structure, and the final metal laminate material contains a metal B layer as a reinforcement.
[0126] In another preferred embodiment of the present invention, a metal laminate material with a single gradient graded porous structure prepared by the aforementioned method is also provided. The metal laminate material has a porous structure, and the pore size in the porous structure presents a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.
[0127] In an optional embodiment, the pore size varies in a gradient, and the minimum average pore size is 20 nm to 50 nm, and the maximum average pore size is 200 nm to 500 nm.
[0128] For better understanding, the present invention is further described below in conjunction with specific examples, but the preparation method is not limited thereto, and the content of the present invention is not limited thereto.
[0129] Unless otherwise specified, the raw materials in the following examples were purchased from commercial sources.
[0130] Example 1
[0131] Similar elements
[0132] (1) The raw materials are metal copper foil and metal silver foil (purity: 99%, thickness of the metal copper foil and the metal silver foil are both 50 μm).
[0133] (2) The metal foil in step (1) is washed in 75% alcohol for 5 minutes at 25° C. in a water bath using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0134] (3) stacking the metal foils treated in step (2) in the order of Cu-Ag-Cu, placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 500°C (Cu melting point: 1083.4°C, Ag melting point: 961.6°C);
[0135] Among them, at 500℃, the diffusion coefficient of Ag in Cu is 10 -12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, argon protection is introduced into the vacuum hot pressing furnace to prevent high-temperature oxidation. According to formula (1), the expected thickness is 5μm, and the required insulation time is estimated to be 0.8h. The purpose is to connect the dissimilar metals with the high-temperature diffusion layer to play a bonding role.
[0136] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by an argon atmosphere to prevent high-temperature oxidation, and heat treated at 500° C. in a muffle furnace, wherein at 500° C., the diffusion coefficient of Ag in Cu is 10 - 12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, according to formula (1), the expected thickness is 60μm, and the required insulation time is estimated to be 1h. The actual infinite solid solution layer thickness is obtained through EDS test and adjusted, and the required insulation time is 60h.
[0137] (5) The laminated material treated in step (4) is subjected to chemical dealloying treatment by being placed in 0.8M HNO3 for chemical dealloying and placed in a water bath at 60°C for 1.5 hours to dissolve Cu and obtain porous Ag.
[0138] Example 2
[0139] Different groups of elements that can form infinite solid solutions
[0140] (1) The raw materials are metal aluminum foil and metal zinc foil (purity: 99%, the thickness of the metal aluminum foil and the metal zinc foil are both 50 μm).
[0141] (2) The metal foil in step (1) is washed in 75% alcohol for 5 minutes at 25° C. in a water bath using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0142] (3) stacking the metal foils treated in step (2) in the order of Zn-Al-Zn, placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 370°C (Al melting point: 660°C, Zn melting point: 419.53°C);
[0143] Among them, at 370℃, the diffusion coefficient of Zn in Al is 10 -13.5 m 2 / s, the diffusion coefficient of Al in Zn is 10 -12.5 m 2 / s, argon protection is introduced into the vacuum hot pressing furnace to prevent high-temperature oxidation. According to formula (1), the thickness of 5 μm is calculated, and the required insulation time is 0.5 h. The purpose is to connect the dissimilar metals in the high-temperature diffusion layer to play a bonding role.
[0144] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by a nitrogen atmosphere to prevent oxidation, and heat treated in a muffle furnace at a temperature controlled at 370° C., wherein at 370° C., the diffusion coefficient of Zn in Al is 10 -13.5 m 2 / s, the diffusion coefficient of Al in Zn is 10 -12.5 m 2 / s, according to formula (1), the thickness of 70μm is calculated, and the required holding time is 10h. The actual infinite solid solution layer thickness at this time is obtained through EDS test and adjusted to obtain a thickness of 70μm, and the required holding time is 80h.
[0145] (5) The laminated material in step (4) is subjected to chemical dealloying treatment by immersing it in 0.01M NaOH for chemical dealloying, placing it in a water bath at 25°C for 8 hours to dissolve Al and obtain porous Zn.
[0146] Example 3
[0147] (1) The raw materials are metal copper foil and metal silver foil (purity: 99%, thickness of the metal copper foil and the metal silver foil are both 50 μm).
[0148] (2) The metal foil in step (1) is washed in 75% alcohol for 5 minutes at 25° C. in a water bath using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0149] (3) stacking the metal foils treated in step (2) in the order of Cu-Ag-Cu-...-Ag, a total of 10 layers, and placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 500°C (Cu melting point: 1083.4°C, Ag melting point: 961.6°C);
[0150] Among them, at 500℃, the diffusion coefficient of Ag in Cu is 10 -12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, argon gas is introduced into the vacuum hot pressing furnace to prevent high-temperature oxidation. According to formula (1), the thickness of 5 μm is calculated, and the required insulation time is 0.8 h. The purpose is to connect the dissimilar metals with the high-temperature diffusion layer to play a bonding role.
[0151] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by an argon atmosphere to prevent high-temperature oxidation, and heat treated at 500° C. in a muffle furnace, wherein at 500° C., the diffusion coefficient of Ag in Cu is 10 - 12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, according to formula (1), the expected thickness is 56μm, and the required holding time is 1h. The actual infinite solid solution layer thickness is obtained through EDS test and adjusted, and the actual required holding time is 60h.
[0152] (5) The laminated material after the treatment in step (4) is subjected to chemical dealloying treatment. First, the metal laminated material in step (4) is brittlely broken by liquid nitrogen, and then placed in 0.8M HNO3 for chemical dealloying. The material is placed in a water bath at 60°C for chemical dealloying for 1.5 hours to dissolve Cu and obtain porous Ag.
[0153] Comparative Example 1
[0154] The same materials and number of layers as in Example 1 are used.
[0155] (1) The raw materials are metal copper foil and metal silver foil (purity: 99%, thickness of the metal copper foil and the metal silver foil are both 50 μm).
[0156] (2) The metal foil in step (1) is washed in 75% alcohol in a water bath at 25° C. for 5 minutes using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0157] (3) stacking the metal foils treated in step (2) in the order of Cu-Ag-Cu, placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 900°C (Cu melting point: 1083.4°C, Ag melting point: 961.6°C);
[0158] Among them, at 900℃, the diffusion coefficient of Ag in Cu is 10 -16.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -14.5 m 2 / s, argon gas is introduced into the vacuum hot pressing furnace to prevent high temperature oxidation. According to formula (1), the thickness of 6 μm is expected, and the required insulation time is calculated to be 10 h. The purpose is to connect the dissimilar metals in the high temperature diffusion layer to play a bonding role.
[0159] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by an argon atmosphere to prevent high-temperature oxidation, and heat treated at 900° C. in a muffle furnace, wherein at 900° C., the diffusion coefficient of Ag in Cu is 10 - 12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, according to formula (1), the thickness is calculated to be 56 μm, and the required insulation time is 0.5 h.
[0160] In Comparative Example 1, the actual holding time is 10 hours. However, since the holding temperature exceeds the softening temperature of the metal, the metallic silver softens under a certain pressure and flows out of the mold gap, so that the solid form of the metal base cannot be maintained and the expected lamination cannot be obtained.
[0161] Comparative Example 2
[0162] (1) The raw materials are metal copper foil and metal silver foil (purity: 99%, thickness of the metal copper foil and the metal silver foil are both 50 μm).
[0163] (2) The metal foil in step (1) is washed in 75% alcohol for 5 minutes at 25° C. in a water bath using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0164] (3) stacking the metal foils treated in step (2) in the order of Cu-Ag-Cu, placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 500°C (Cu melting point: 1083.4°C, Ag melting point: 961.6°C);
[0165] Among them, at 500℃, the diffusion coefficient of Ag in Cu is 10 -12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, argon protection is introduced into the vacuum hot pressing furnace to prevent high-temperature oxidation. According to formula (1), the expected thickness is 5μm, and the required insulation time is estimated to be 0.8h. The purpose is to connect the dissimilar metals with the high-temperature diffusion layer to play a bonding role.
[0166] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by an argon atmosphere to prevent high-temperature oxidation, and heat treated at 500° C. in a muffle furnace, wherein at 500° C., the diffusion coefficient of Ag in Cu is 10 - 12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, according to formula (1), if the desired thickness is 10 μm, the required insulation time is estimated to be 1.6 h.
[0167] (5) The laminated material treated in step (4) is subjected to chemical dealloying treatment by being placed in 0.8M HNO3 for chemical dealloying and placed in a water bath at 60°C for 1.5 hours to dissolve Cu and obtain porous Ag.
[0168] In Comparative Example 2, the actual holding time was 2.4 h. However, since the diffusion layer generated during the holding time was too thin, it was placed in 0.8 M HNO3 for chemical dealloying. During the experiment, the metal foil peeled off, so that the expected lamination could not be obtained.
[0169] Comparative Example 3
[0170] (1) The raw materials are metal copper foil and metal silver foil (purity: 99%, thickness of the metal copper foil and the metal silver foil are both 50 μm).
[0171] (2) The metal foil in step (1) is washed in 75% alcohol in a water bath at 25° C. for 5 minutes using a numerically controlled ultrasonic cleaner to eliminate any oily impurities that may exist on the surface of the metal foil.
[0172] (3) stacking the metal foils treated in step (2) in the order of Cu-Ag-Cu, placing them in a vacuum hot pressing furnace mold, applying a pressure of 5 MPa in the vacuum hot pressing furnace, and controlling the temperature at 500°C (Cu melting point: 1083.4°C, Ag melting point: 961.6°C);
[0173] Among them, at 500℃, the diffusion coefficient of Ag in Cu is 10-12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, argon protection is introduced into the vacuum hot pressing furnace to prevent high-temperature oxidation. According to formula (1), the expected thickness is 5μm, and the required insulation time is estimated to be 0.8h. The purpose is to connect the dissimilar metals with the high-temperature diffusion layer to play a bonding role.
[0174] (4) The laminated material after the treatment in step (3) is passed through a vacuum quartz sealing tube, protected by an argon atmosphere to prevent high-temperature oxidation, and heat treated at 500° C. in a muffle furnace, wherein at 500° C., the diffusion coefficient of Ag in Cu is 10 - 12.5 m 2 / s, the diffusion coefficient of Cu in Ag is 10 -11.75 m 2 / s, according to formula (1), the expected thickness is 127μm, and the required insulation time is estimated to be 5h. The actual infinite solid solution layer thickness is obtained through EDS test and adjusted, and the required insulation time is 200h.
[0175] (5) The laminated material treated in step (4) is subjected to chemical dealloying treatment by being placed in 0.8M HNO3 for chemical dealloying and placed in a water bath at 60°C for 1.5 hours to dissolve Cu and obtain porous Ag.
[0176] In Comparative Example 3, the actual insulation time is 200h, but due to the long insulation time, the diffusion layer is too thick, exceeding 100μm. After it is put into 0.8M HNO3 for chemical dealloying, there is no pure inert metal layer in the obtained porous material, and the laminated material with the expected structure cannot be obtained.
[0177] SEM Testing
[0178] SEM test was performed on the samples in Example 1 and Example 2.
[0179] like Figure 4 As shown, when metal Cu and Ag foils are stacked together, there will be an obvious physical interface between the metal foils;
[0180] Figure 5 Mapping data description, Figure 4 After the stacked metal is heat treated, the atoms diffuse into each other to form a diffusion layer with both Cu and Ag. Figure 4 It can be seen that the process causes atomic thermal diffusion and breaks the physical interface. The red part is the Cu element and the green part is the Ag element. Figure 5 a is the cross-sectional diagram of the CuAg stack thermal diffusion. Figure 5 b. Figure 5 c. Figure 5 d The three figures are all to illustrate the distribution of elements, combined with the table Figure 6 From the energy spectrum line scan data and Table 1, it can be concluded that the specific diffusion layer is 40μm.
[0181] Table 1 Element distribution of CuAg cross section
[0182]
[0183] like Figure 7 , Figure 8 As shown, through dealloying, Cu atoms are dissolved to obtain porous Ag.
[0184] Figure 7 This is the morphology of the sample cross section after the CuAg stack was chemically dealloyed by heat treatment. Figure 7 a is the overall shape, Figure 7 b. Figure 7 c. Figure 7 d are Figure 7 From the high-magnification morphology images at different positions on a, it can be seen that due to the different atomic distribution when CuAg atoms diffuse, the porous morphology obtained by chemical dealloying is different.
[0185] Figure 8 This is the morphology of the sample surface after the CuAg stack was chemically dealloyed by heat treatment. Figure 8 a is the overall shape, Figure 8 b. Figure 8 c. Figure 8 d are Figure 8 From the high-magnification morphology image at the same position in a, it can be seen that due to the different atomic distribution when CuAg atoms diffuse to, the porous morphology obtained by chemical dealloying on the diffusion path is the same.
[0186] like Fig. 9 As shown, Fig. 9 a is the overall shape, Fig. 9 b. Fig. 9 c. Fig. 9 d are Fig. 9 High-magnification morphology at different positions on a. It can be seen from the figure that the metal Zn and Al foil are superimposed together. After the laminated metal is heat treated, the atoms diffuse into each other to form a diffusion layer containing both Zn and Al. The process causes the atoms to diffuse thermally and breaks the physical interface. Through dealloying, Al atoms are dissolved to obtain porous Zn. Due to the different atomic distributions when AlZn atoms diffuse, the porous morphology is obtained through chemical dealloying. The influence of different oxygen atoms makes the surface of the AlZn laminate present a petal-like structure.
[0187] This indicates that the metal laminate material with a single gradient hierarchical porous structure is successfully prepared by the method of the present invention.
[0188] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.
Claims
1. A method for preparing a metal laminate material having a single gradient hierarchical porous structure, characterized in that: The following steps are involved: S1. Cleaning the surfaces of the first metal and the second metal to remove processing oil and other impurities on the metal surfaces; wherein there are differences in chemical activity and thermodynamic stability between the first metal and the second metal, and it is defined that the first metal is more active than the second metal, and the diffusion rate of the first metal is faster than that of the second metal; S2, after the first metal and the second metal cleaned in step S1 are sequentially stacked N times, a diffusion welding additive manufacturing process is used to eliminate the physical interface between the first metal and the second metal, so that the first metal and the second metal are tightly combined to obtain a first intermediate; wherein N≥1; The specific process of the diffusion welding additive manufacturing process is as follows: The first metal and the second metal cleaned in step S1 are sequentially stacked on each other and placed in a vacuum hot pressing furnace, the pressure is applied to 5-20 MPa, and the temperature is controlled to T1, and the first heat preservation treatment is performed under the protection of nitrogen atmosphere until the physical interface between the first metal and the second metal is eliminated; wherein the control range of temperature T1 is 0.5T m ≤T1<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal; S3, heat-treating the first intermediate so that the first metal and the second metal diffuse into each other to form an infinite solid solution, thereby obtaining a second intermediate; wherein the second intermediate comprises a second metal layer and an infinite solid solution layer; The value of the thickness X of the required infinite solid solution layer is: W<X<2W; wherein W is the relatively larger thickness value between the thickness of the first metal and the thickness of the second metal; the thickness Y of the first metal is 3μm~200μm, and the thickness Z of the second metal is 3μm~200μm; The heat treatment process is as follows: The first intermediate is sealed by a vacuum quartz tube, protected by a nitrogen atmosphere, placed in a muffle furnace, and subjected to a second heat preservation treatment at a temperature of T2; wherein the temperature T2 is set according to the requirement of forming an infinite solid solution layer; and the time of the second heat preservation treatment is set according to the required thickness X of the infinite solid solution layer; The control range of temperature T2 is 0.5T m ≤T2<T 软 , when the melting point of the first metal is greater than the melting point of the second metal, T m is the melting point of the second metal, T 软 is the softening temperature of the second metal; when the melting point of the first metal is lower than the melting point of the second metal, T m is the melting point of the first metal, T 软 is the softening temperature of the first metal; The time of the second heat preservation treatment is determined as follows: According to formula (1), the time t of the second heat preservation treatment without heat loss is obtained: (1) Where X is the thickness of the required infinite solid solution layer, m; X1 is the diffusion thickness of the first metal in the second metal, m; X2 is the diffusion thickness of the second metal in the first metal, m; t is the time of the second insulation treatment without heat loss, s; D1 is the diffusion coefficient of the first metal in the second metal, m 2 / s; D2 is the diffusion coefficient of the second metal in the first metal, m 2 / s; Heat preservation is performed at time t to obtain an infinite solid solution layer with a thickness of X'. When X'<X, the time of the second heat preservation treatment is increased until the thickness of the infinite solid solution layer meets the requirements; when X'>X, the time of the second heat preservation treatment is reduced until the thickness of the infinite solid solution layer meets the requirements; S4, subjecting the second intermediate to dealloying treatment to remove the first metal atoms in the infinite solid solution layer, thereby forming a porous structure and obtaining a metal laminate material; Among them, in the porous structure, the pore size shows a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.
2. The method for preparing a metal laminate material having a single gradient hierarchical porous structure according to claim 1, characterized in that: The first metal and the second metal are two metals in the same group of elements.
3. The method for preparing a metal laminate material having a single gradient hierarchical porous structure according to claim 1, characterized in that: When N=1, in the porous structure, the pore size presents a single gradient change from small to large along the second metal layer toward one side.
4. The method for preparing a metal laminate material having a single gradient hierarchical porous structure according to claim 1, characterized in that: When N>1, in the porous structure, the pore diameter presents a single gradient change from small to large along the second metal layer toward both sides.
5. A metal laminate material having a single gradient hierarchical porous structure prepared by the method according to any one of claims 1 to 4, characterized in that: The metal laminate material has a porous structure, and the pore diameter in the porous structure presents a single gradient change from small to large along the second metal layer toward the outside, thereby forming a single gradient graded porous structure.