By using ethoxy end capping polymers and chain extenders in single-component deethanol-type silicone sealants, the problem of insufficient methanol release and chain extenders is solved, and an environmentally friendly and healthy curing process and low-cycle silicone are achieved. The content of oxane meets the environmental protection requirements of EU standards.

CN117210192BActive Publication Date: 2024-11-12JIANGXI BLUESTAR XINGHUO SILICONE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311176141.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2024-11-12
Estimated Expiration
2043-09-13

AI Technical Summary

Technical Problem

The existing single-component dealcoholized silicone sealant will release methanol during the curing process, which is not environmentally friendly enough, the chain extender is not active enough, the preparation is difficult and the environmental pollution is high, the content of D3 to D10 is high, and it does not meet the environmental protection. standard.

Method used

Using a single component deethanol-type silicone sealant composition, including ethoxy end capping polymer and ethoxy end capping chain extender, the avoidance and chain extension effect of methanol release is achieved by controlling the degree of polymerization and viscosity, and the chain extension effect is reduced. Cyclosiloxane content, complies with SVHC standards.

Benefits of technology

The methanol does not release during the curing process, which improves environmental protection, simplifies the preparation of chain extenders, reduces the cyclosiloxane content, meets the EU's environmental protection requirements, and is suitable for indoor and outdoor decoration and electronic and electrical products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

This invention relates to a one-component, alcohol-free silicone sealant composition and its preparation method. The sealant composition comprises 100 parts by weight of a base adhesive, 1-150 parts by weight of a reinforcing filler, 1-10 parts by weight of a crosslinking agent, and 0.01-5 parts by weight of a catalyst. The base adhesive comprises an ethoxylated end-capped polymer and an ethoxylated end-capped chain extender. The ethoxylated end-capped polymer includes at least one polymer selected from those shown in Formula I and Formula II, and the ethoxylated end-capped chain extender includes a polymer shown in Formula III. The weight ratio of the ethoxylated end-capped polymer to the ethoxylated end-capped chain extender is 8:2 to 5:5. The one-component, alcohol-free silicone sealant composition of this invention does not release methanol during curing, making it more environmentally friendly and healthier for both indoor and outdoor decoration and electronic and electrical products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic silicon sealants, and in particular relates to a single-component deethanol type organic silicon sealant composition and a preparation method thereof. Background Art

[0002] Single-component dealcoholization silicone sealants are widely used in various industries such as electronics, 5G communications, road traffic, new energy, automobiles, curtain wall doors and windows, aerospace, etc. Due to technical reasons, low-modulus single-component dealcoholization silicone sealants are relatively rare on the market, and low-modulus single-component deethanolization silicone sealants are even rarer. Whether it is used for home decoration building materials or in electronics and electrical fields, the environmental performance of deethanolization silicone sealants is more advantageous.

[0003] Chinese patent CN108822790B discloses a one-component dealcoholized low modulus silicone weatherproof sealant and its preparation method, which belongs to the field of silicone weatherproof sealant, including α,ω-dihydroxy polydimethylsiloxane, calcium carbonate, thixotropic agent, dimethyl silicone oil, chain extender, crosslinking agent, coupling agent and catalyst, the chain extender includes a first chain extender and a second chain extender, the first chain extender is a silane oligomer, and the second chain extender is a long-chain carbon siloxy solid silane. In the preparation process, the order of adding the crosslinking agent, the first chain extender and the second chain extender is: the first chain extender, the crosslinking agent and the second chain extender. The patent selects a suitable chain extender and improves the preparation process to obtain an environmentally friendly, short surface drying time, low modulus, and high elongation one-component dealcoholized silicone sealant, which is suitable for sealing of concrete expansion joints of super high-rise buildings, large concrete facilities, roads, bridges, airport runways and other facilities, meeting the requirements of the industry and the market.

[0004] Chinese patent CN103436216B provides a dealcoholization type low modulus and high elongation silicone sealant and a preparation method thereof. The silicone sealant is composed of 100 parts of a base polymer, 5-30 parts of a plasticizer, 5-150 parts of a filler, 1-15 parts of a cross-linking agent, 1-5 parts of a thixotropic agent, 0.2-3 parts of a stabilizer, 0.5-3 parts of a catalyst, and 0.5-3 parts of a coupling agent. During preparation, the above raw materials are added into a high-speed disperser at a vacuum degree of 0.06-0.095 MPa and a rotation speed of 20-600 rpm for a chemical reaction for 60-180 minutes. The silicone sealant of the patent has low modulus and high elongation, good elastic recovery rate, good aging resistance and high and low temperature performance.

[0005] Chinese patent application CN114214026A discloses a dealcoholization type high elasticity low modulus silicone sealant and its preparation method. The dealcoholization type high elasticity low modulus silicone sealant is made of the following raw materials: nano calcium carbonate, 107 base glue, silicone oil, fumed silica, a first crosslinking agent, a second crosslinking agent, a coupling agent and a titanium catalyst; the preparation method comprises the following steps: S1, at 110-150°C, nano calcium carbonate, 107 base glue and silicone oil are mixed and stirred to obtain a mixture A; S2, mixture A is cooled to 25-30°C, the second crosslinking agent is added, and the mixture is mixed and stirred; S3, the first crosslinking agent is added, and the mixture is mixed and stirred; S4, the fumed silica is added, and the mixture is mixed and stirred; S5, the coupling agent and the catalyst are added to the mixed and stirred materials in S4, the mixture is mixed and stirred, and the finished product is obtained by filling. The product of Chinese patent application CN114214026A has the advantage of improving the curing rate of the dealcoholization type silicone sealant.

[0006] Chinese patent application CN113897171A discloses a high displacement dealcoholization flame retardant fireproof sealant and its preparation method. The raw materials of the high displacement dealcoholization flame retardant fireproof sealant include 100 parts of α,ω-dihydroxy polydimethylsiloxane, 5-10 parts of dealcoholization chain extender, 30-60 parts of reactive plasticizer, 50-100 parts of calcium carbonate, 40-90 parts of ultrafine modified flame retardant filler, 25-55 parts of dealcoholization curing agent, 5-20 parts of thixotropic agent and 1 part of first catalyst, by weight. The sealant of Chinese patent application CN113897171A has excellent chemical stability, weathering resistance, thixotropy and construction performance, and can be used as a sealing material for building curtain walls.

[0007] Chinese patent CN108179003B discloses a dealcoholized silicone weatherproof sealant and its preparation method. The silicone weatherproof sealant is prepared from the following raw materials by weight: 100 parts of methyl dimethoxy-terminated 107 glue, 0-40 parts of dimethyl silicone oil, 10-40 parts of monohydroxy silicone oil, 60-200 parts of inorganic filler, 2-10 parts of compound crosslinking agent, 0.5-3 parts of silane coupling agent, and 0.05-0.5 parts of catalyst; the compound crosslinking agent is selected from at least two of methyl trimethoxysilane, methyl triethoxysilane, methyl tripropoxysilane, methyl orthosilicate, ethyl orthosilicate, isopropyl orthosilicate, dimethyl dimethoxysilane, dimethyl diethoxysilane and dimethyl dipropoxysilane. The silicone weatherproof sealant has a lower modulus and a high level of displacement capacity, has low stress on curtain wall panels, and has excellent weather resistance and good adhesion and water resistance.

[0008] However, the single-component dealcoholized silicone sealants of current technology have one or more of the following problems:

[0009] (1) The glue releases methanol during the curing process, which is not environmentally friendly;

[0010] (2) The activity of the chain extender is not high enough, and the chain extension effect is not obvious during the curing process of the glue;

[0011] (3) Chain extenders are difficult to purchase and difficult to prepare, and the preparation process causes significant environmental pollution;

[0012] (4) D3~D10 have high cyclosiloxane content and are not environmentally friendly. Summary of the invention

[0013] Therefore, the purpose of the present invention is to provide a one-component deethanol type silicone sealant composition and a preparation method thereof in view of the problems existing in the prior art. The one-component deethanol type silicone sealant composition of the present invention does not release methanol during the curing process, and is more environmentally friendly and healthy whether used for indoor and outdoor decoration or electronic and electrical products.

[0014] The objectives of the present invention are achieved through the following technical solutions.

[0015] In a first aspect, the present invention provides a one-component deethanol-type silicone sealant composition, wherein the sealant composition comprises 100 parts by weight of a base glue, 1 to 150 parts by weight of a reinforcing filler, 1 to 10 parts by weight of a cross-linking agent, and 0.01 to 5 parts by weight of a catalyst; wherein the base glue comprises an ethoxy-terminated polymer and an ethoxy-terminated chain extender, wherein the ethoxy-terminated polymer comprises at least one selected from the group consisting of polymers represented by formula I and formula II, wherein the ethoxy-terminated chain extender comprises a polymer represented by formula III, and wherein the weight ratio of the ethoxy-terminated polymer to the ethoxy-terminated chain extender is 8:2 to 5:5;

[0016]

[0017] In formula I, R1 and R2 are the same or different and are independently selected from methyl, ethyl and phenyl; R3 is selected from methyl, vinyl, diethylaminomethyl, anilinomethyl, aminopropyl, aminoethylaminopropyl (e.g., N-(β-aminoethyl)-γ-aminopropyl) and ethoxy; m ranges from 100 to 5000;

[0018]

[0019] In formula II, R4 and R5 are the same or different and are independently selected from methyl, ethyl and phenyl; R6 is selected from methyl and ethoxy; X is -CH2CH2-; n is in the range of 100 to 5000;

[0020]

[0021] In formula III, R7 is selected from diethylaminomethyl, dichloromethyl and anilinemethyl; R8 is selected from methyl, propyl, vinyl and -O-Si(CH3)3; and a ranges from 10 to 3000.

[0022] In the one-component deethanol type silicone sealant composition of the present invention, specific ethoxy-terminated polymers and ethoxy-terminated chain extenders are selected as the base glue, and methanol is not released during the curing process. It can be used for indoor and outdoor decoration or electronic and electrical products, which is more environmentally friendly and healthy. Furthermore, compared with the common silicon-ethoxy group containing only one ethoxy group at each end, which has a low hydrolysis activity and is difficult to play a chain extension role, the ethoxy-terminated chain extender of formula III defined in the present invention has a high hydrolysis activity of the ethoxy group. The ethoxy-terminated chain extender shown in formula III can achieve a good chain extension effect during the curing process, so that the glue has a higher elongation at break after curing. It is believed that such hydrolysis activity is caused by R7. In addition, the ethoxy-terminated chain extender also shows a certain plasticizing effect, so that the composition of the present invention can be free of plasticizers and can also keep the composition at a suitable viscosity.

[0023] According to the one-component deethanol-type organosilicon sealant composition provided by the present invention, the content of cyclosiloxane in the sealant composition is less than 1000 ppm.

[0024] In the present invention, the term "cyclosiloxane" refers to D3-D10 siloxane ring bodies.

[0025] The present invention controls the content of cyclosiloxane in the sealant composition to be lower than 1000 ppm, thereby meeting the SVHC standard for export to the European Union.

[0026] According to the one-component alcohol-free silicone sealant composition provided by the present invention, the viscosity of the ethoxy-terminated polymer at 25° C. is 500 to 100,000 cps. In the present invention, if the viscosity of the ethoxy-terminated polymer is too high, it is not conducive to the use of the sealant composition; conversely, if the viscosity is too low, the mechanical properties of the sealant composition are reduced.

[0027] On the one hand, the present invention can control the viscosity of the ethoxy-terminated polymers shown in formula I and formula II by controlling the m and n values ​​(polymerization degree). On the other hand, the present invention can also replace the m and n values ​​in formula I and formula II by limiting the viscosity of the ethoxy-terminated polymers. To a certain extent, the polymerization degrees m and n can be reflected by viscosity.

[0028] In some embodiments, the viscosity of the ethoxy terminated polymer at 25° C. may be 500 cps, 750 cps, 1000 cps, 1500 cps, 2000 cps, 3000 cps, 4000 cps, 5000 cps, 8000 cps, 10000 cps, 20000 cps, 30000 cps, 40000 cps, 50000 cps, 60000 cps, 80000 cps, 100000 cps, or a range consisting thereof.

[0029] In other embodiments, m ranges from 200 to 2000; and / or n ranges from 200 to 2000.

[0030] According to the one-component alcohol-free silicone sealant composition provided by the present invention, the viscosity of the ethoxy-terminated chain extender at 25° C. is 10 to 50,000 cps. Similarly, in the present invention, if the viscosity of the ethoxy-terminated chain extender is too high, it may be detrimental to the use of the sealant composition; conversely, if the viscosity is too low, the mechanical properties of the sealant composition may be reduced.

[0031] On the one hand, the present invention can control the viscosity of the ethoxy-terminated chain extender by controlling the a value (polymerization degree) in the formula III. On the other hand, the present invention can replace the a value in formula III by limiting the viscosity of the ethoxy-terminated chain extender. To a certain extent, the polymerization degree a can be reflected by viscosity.

[0032] In some embodiments, the viscosity of the ethoxy capped chain extender at 25° C. can be 10 cps, 20 cps, 50 cps, 100 cps, 150 cps, 200 cps, 300 cps, 400 cps, 500 cps, 800 cps, 1000 cps, 2000 cps, 5000 cps, 8000 cps, 10000 cps, 20000 cps, 30000 cps, 40000 cps, 50000 cps, or a range composed thereof.

[0033] In other embodiments, a ranges from 50 to 1500.

[0034] According to the one-component deethanolic silicone sealant composition provided by the present invention, the weight ratio of the ethoxy-terminated polymer to the ethoxy-terminated chain extender can be 8:2, 7:3, 6:4, 5:5 or a range thereof. If the ethoxy-terminated chain extender in the sealant composition is too low, the chain extension effect is not obvious, and the elongation of the sealant after curing cannot be significantly improved; conversely, if the ethoxy-terminated chain extender in the sealant composition is too high, it is difficult for the sealant to form a sufficient number of cross-linked network structures after curing, and the strength is low, the hardness is too low, the modulus is too low, and the elongation at break cannot be significantly improved, and the surface drying of the sealant may be slow or even not cured.

[0035] According to the one-component deethanolic silicone sealant composition provided by the present invention, the ethoxy-terminated polymer shown in Formula I can be prepared by a condensation reaction between a silane crosslinker containing at least two ethoxy groups and a terminal hydroxyl polysiloxane.

[0036] The ethoxy-terminated polymer shown in formula II can be prepared by a hydrosilylation reaction between a hydrogen-containing ethoxysilane and a vinyl-terminated polysiloxane, or by a hydrosilylation reaction between a vinyl-containing ethoxysilane and a hydrogen-terminated polysiloxane.

[0037] According to the one-component alcohol-free silicone sealant composition provided by the present invention, the ethoxy-terminated chain extender represented by formula III can be prepared by a condensation reaction between a corresponding end-capping agent and a hydroxy-terminated polysiloxane.

[0038] In the present invention, the terminal hydroxyl polysiloxane may be α,ω-dihydroxy polydimethylsiloxane (107 glue), preferably α,ω-dihydroxy polydimethylsiloxane with a D3-D10 siloxane ring body content of less than 1000ppm. The ethoxy-terminated polymer and ethoxy-terminated chain extender prepared by using α,ω-dihydroxy polydimethylsiloxane with a siloxane ring body content of less than 1000ppm, the cyclosiloxane content of the finally prepared deethanolic silicone sealant meets the SVHC standard.

[0039] According to the one-component deethanolic silicone sealant composition provided by the present invention, the reinforcing filler is selected from precipitated silica, fumed silica, hydrophobic treated silica, nano-activated calcium carbonate, heavy calcium carbonate, carbon nanotubes, graphene, glass fiber, silicate, nano-montmorillonite and mixtures thereof.

[0040] In some embodiments, the reinforcing filler is selected from precipitated silica, fumed silica and hydrophobically treated silica, and the amount of the reinforcing filler is 1 to 30 parts by weight.

[0041] In some embodiments, the reinforcing filler is selected from nano-active calcium carbonate and heavy calcium carbonate, and the amount of the reinforcing filler is 50 to 150 parts by weight, for example, 90 parts by weight.

[0042] According to the one-component deethanol-type silicone sealant composition provided by the present invention, the crosslinking agent is selected from tetraethyl orthosilicate, polyethyl orthosilicate, methyltriethoxysilane, vinyltriethoxysilane, 3-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane and mixtures thereof.

[0043] According to the one-component deethanol-type silicone sealant composition provided by the present invention, the amount of the cross-linking agent can be 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight or a range thereof.

[0044] According to the one-component alcohol-free silicone sealant composition provided by the present invention, the catalyst is selected from organotin, organotin chelate, titanate, titanate chelate, organobismuth, aminosilane and mixtures thereof. In some embodiments, the catalyst is selected from titanate catalyst, titanate complex, dibutyltin dilaurate, dibutyltin diacetate and mixtures thereof.

[0045] According to the one-component deethanol type silicone sealant composition provided by the present invention, the amount of the catalyst can be 0.01 weight part, 0.05 weight part, 0.1 weight part, 0.2 weight part, 0.3 weight part, 0.4 weight part, 0.5 weight part, 0.8 weight part, 1 weight part, 2 weight parts, 3 weight parts, 4 weight parts, 5 weight parts or a range thereof.

[0046] According to the one-component alcohol-free organic silicon sealant composition provided by the present invention, the sealant composition further comprises:

[0047]

[0048] According to the one-component deethanol type silicone sealant composition provided by the present invention, the flame retardant filler is selected from aluminum hydroxide, magnesium hydroxide, carbon (graphite) flame retardant, nitrogen-phosphorus flame retardant, phosphorus-silicon flame retardant, platinum-containing flame retardant and mixtures thereof.

[0049] According to the one-component alcohol-free silicone sealant composition provided by the present invention, the thermally conductive filler is selected from aluminum hydroxide, aluminum oxide, zinc oxide, cerium oxide, aluminum nitride, boron nitride, silicon nitride, silicon carbide, graphene, carbon nanotubes, quartz powder, aluminum powder, copper powder, silver powder and mixtures thereof. In the present invention, the thermally conductive filler is preferably subjected to hydrophobic treatment.

[0050] According to the one-component deethanol type silicone sealant composition provided by the present invention, the coupling agent is selected from 3-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane, dodecyltriethoxysilane, hexadecyltriethoxysilane, anilinemethyltriethoxysilane and mixtures thereof.

[0051] According to the one-component alcohol-free organosilicon sealant composition provided by the present invention, the plasticizer is selected from methyl silicone oil, phenyl silicone oil, vinyl silicone oil and a mixture thereof.

[0052] In the present invention, the viscosity of the plasticizer at 25° C. may range from 0.5 to 1000 cps, preferably from 1 to 500 cps.

[0053] In a second aspect, the present invention provides a method for preparing a one-component deethanol-type silicone sealant composition, wherein the preparation method comprises the following steps: mixing a base glue, a reinforcing filler, a cross-linking agent, a catalyst, an optional flame retardant filler, an optional thermal conductive filler, an optional coupling agent, an optional pigment and an optional plasticizer uniformly in a moisture-proof environment, and stirring the mixture at a temperature of 10 to 60° C., preferably 20 to 50° C. and a negative pressure of -0.085 to -0.099 MPa for 15 to 180 min, preferably 20 to 60 min, and optionally cooling the mixture to room temperature to obtain a one-component deethanol-type silicone sealant composition.

[0054] According to the preparation method provided by the present invention, the powder raw material of the single-component deethanol type silicone sealant composition can be pre-treated for dehydration.

[0055] According to the preparation method provided by the present invention, the preparation method of the ethoxy-terminated polymer shown in Formula I comprises the following steps:

[0056] S100, at a temperature of 10 to 150° C., preferably 20 to 40° C., under the protection of an inert gas and in the presence of an optional condensation catalyst, a silane crosslinking agent A containing at least two ethoxy groups is subjected to a condensation reaction with a terminal hydroxyl polysiloxane.

[0057] Preferably, the condensation reaction time in step S100 is 2-36 h, preferably 18-36 h, for example, 24 h.

[0058] Preferably, the structure of the silane crosslinking agent A containing at least two ethoxy groups in step S100 is as shown in Formula IV,

[0059]

[0060] In formula IV, R3 is selected from methyl, vinyl, diethylaminomethyl, phenylaminomethyl, aminopropyl, aminoethylaminopropyl and ethoxy; R 10 It is ethyl.

[0061] Preferably, the condensation catalyst in step S100 is butanone oxime; and / or, based on the weight of the hydroxy-terminated polysiloxane, the amount of the condensation catalyst is 0.001 to 1% by weight.

[0062] In the present invention, in step S100, the weight ratio of the terminal hydroxyl polysiloxane to the silane crosslinking agent A containing at least two ethoxy groups is 100:(1-20), preferably 100:(1-10).

[0063] Preferably, the inert gas in step S100 is nitrogen, helium or argon.

[0064] In the present invention, the structure of the hydroxy-terminated polysiloxane in step S100 can be determined according to formula I.

[0065] According to the preparation method provided by the present invention, the preparation method of the ethoxy-terminated polymer shown in Formula II comprises the following steps:

[0066] S200, at a temperature of 10 to 150° C., preferably 20 to 40° C., under the protection of an inert gas and in the presence of an optional addition-type catalyst, a silane crosslinking agent B containing at least two ethoxy groups is subjected to an addition reaction with a terminal vinyl polysiloxane.

[0067] Preferably, the addition reaction time in step S200 is 2-36 h, preferably 18-36 h, for example, 24 h.

[0068] Preferably, the silane crosslinking agent B containing at least two ethoxy groups in step S200 is triethoxysilane or methyldiethoxysilane.

[0069] Preferably, the addition catalyst in step S200 is selected from chloroplatinic acid or Custer platinum catalyst; and / or, based on the weight of the vinyl-terminated polysiloxane, the addition catalyst is used in an amount of 0.0001 to 0.01 wt %.

[0070] Preferably, in step S200, the weight ratio of the terminal vinyl polysiloxane to the silane crosslinking agent B containing at least two ethoxy groups is 100:(1-20), preferably 100:(1-10).

[0071] Preferably, the inert gas in step S200 is nitrogen, helium or argon.

[0072] In the present invention, the silane crosslinking agent B may be the same as the silane crosslinking agent A. In addition, the vinyl-terminated polysiloxane may be determined according to Formula II.

[0073] According to the preparation method provided by the present invention, wherein in formula III, R8 is -O-Si(CH3)3, the preparation method of the ethoxy-terminated chain extender comprises the following steps:

[0074] S310, at a temperature of 10 to 50° C., preferably 20 to 30° C., in a moisture-proof condition, add the same amount of trimethylsilanol to diethylaminomethyltriethoxysilane, anilinemethyltriethoxysilane or dichloromethyltriethoxysilane, react for 90 to 180 minutes, raise the temperature to 50 to 80° C., remove the generated ethanol under negative pressure, and obtain an intermediate product;

[0075] S320, reacting the intermediate product with terminal hydroxyl polysiloxane at a temperature of 10 to 50° C., preferably 20 to 30° C., under the protection of an inert gas for 90 to 180 minutes, then heating to 50 to 80° C., removing the generated ethanol under negative pressure, and obtaining an ethoxy-terminated chain extender.

[0076] Preferably, in step S320, the weight ratio of the intermediate product to the hydroxy-terminated polysiloxane is 2 to 10:100.

[0077] Preferably, the reaction in step S320 can be carried out in the presence of a catalyst. Preferably, the catalyst is selected from organotin, titanate, acid, base, amino compound, butanone oxime.

[0078] More preferably, the amount of catalyst added in step S320 is 0.01-1% of the total weight of the reactants.

[0079] Preferably, the inert gas in step S320 is nitrogen, helium or argon.

[0080] In the present invention, the hydroxy-terminated polysiloxane described in S320 can be determined according to Formula III.

[0081] The terminal hydroxyl polysiloxane in the present invention may be α,ω-dihydroxy polydimethylsiloxane (107 gum), preferably α,ω-dihydroxy polydimethylsiloxane having a D3-D10 siloxane ring content of less than 1000 ppm.

[0082] The viscosity of the α,ω-dihydroxypolydimethylsiloxane suitable for preparing the ethoxy terminated polymer at 25° C. can be 500 cps, 750 cps, 1000 cps, 1500 cps, 2000 cps, 3000 cps, 4000 cps, 5000 cps, 8000 cps, 10000 cps, 20000 cps, 30000 cps, 40000 cps, 50000 cps, 60000 cps, 80000 cps, 100000 cps or a range thereof.

[0083] The viscosity of the α,ω-dihydroxy polydimethylsiloxane suitable for preparing the ethoxy-terminated chain extender at 25° C. can be 10 cps, 50 cps, 100 cps, 150 cps, 200 cps, 300 cps, 400 cps, 500 cps, 800 cps, 1000 cps, 2000 cps, 5000 cps, 8000 cps, 10000 cps, 20000 cps, 30000 cps, 40000 cps, 50000 cps or a range thereof.

[0084] α,ω-dihydroxy polydimethylsiloxane can be purchased from the P48 series products of Jiangxi Bluestar Xinghuo Silicone Co., Ltd.; terminal vinyl silicone oil can be purchased from the L621 series products of Jiangxi Bluestar Xinghuo Silicone Co., Ltd.

[0085] The present invention has the following advantages:

[0086] (1) The one-component alcohol-free silicone sealant composition of the present invention does not release methanol during the curing process, can be used for indoor and outdoor decoration or electronic and electrical products, and is more environmentally friendly and healthy.

[0087] (2) The chain extender used in the one-component deethanol-type silicone sealant composition of the present invention is easy to prepare and easy to promote and apply.

[0088] (3) The one-component deethanol-type silicone sealant composition of the present invention has a low content of small molecular siloxane ring bodies, meets the requirements of the EU Reach regulations, is more environmentally friendly, and is easy to export. DETAILED DESCRIPTION

[0089] The present invention is further described below in conjunction with specific embodiments.

[0090] The raw materials used in the examples and comparative examples of the present invention are as follows:

[0091] (1) Polydimethylsiloxane:

[0092]

[0093]

[0094] (2) Ethyl orthosilicate, methyltriethoxysilane, dimethyldiethoxysilane, industrial grade, Hangzhou Guibao Chemical Co., Ltd.;

[0095] (3) Diethylaminomethyltriethoxysilane, anilinemethyltriethoxysilane, dichloromethyltriethoxysilane: Nanjing Jingtianwei Chemical;

[0096] (4) Trimethylsilanol: Aladdin Chemical Reagent Procurement Platform;

[0097] (5) Triethoxysilane (CAS No. 998-30-1): 97%, Aladdin Chemical Reagent Purchasing Platform;

[0098] (6) Trimethoxysilane: 95%, Aladdin Chemical Reagent Purchasing Platform;

[0099] (7) Chloroplatinic acid hexahydrate: Aladdin Chemical Reagent Procurement Platform

[0100] (8) 3-Aminopropyltriethoxysilane: industrial grade, Jingzhou Jianghan Fine Chemical Co., Ltd.;

[0101] (9) N-(β-aminoethyl)-γ-aminopropyltriethoxysilane: industrial grade, Jingzhou Jianghan Fine Chemical Co., Ltd.;

[0102] (10) Dibutyltin dilaurate: Xindian Chemical Materials (Shanghai) Co., Ltd.;

[0103] (11) Calcium carbonate: CCS-25, Guangxi Huana New Materials Co., Ltd.

[0104] (12) Fumed silica: 812S, Evonik Degussa China Ltd.;

[0105] (13) Fumed silica: S150, Cabot Bluestar Chemical (Jiangxi) Co., Ltd.

[0106] Example 1

[0107] 1) 40 parts by weight of P48V80000, 40 parts by weight of P48V20000 and 20 parts by weight of P48V1500 are added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 3 parts by weight of ethyl orthosilicate are added, and the mixture is fully mixed, and then 0.5 parts by weight of butanone oxime is added, and the mixture is continuously stirred under the protection of dry nitrogen, and the temperature is gradually raised to 80° C., reacted for 24 hours, and finally low molecular weights are removed by vacuum, and then the temperature is lowered to room temperature to obtain an ethoxy-terminated polymer, wherein the stirring speed is 500 rpm. In the ethoxy-terminated polymer, R1 and R2 are methyl groups, and R3 is an ethoxy group.

[0108] 2) 100 parts by weight of anilinemethyltriethoxysilane and 1 part by weight of dibutyltin dilaurate were added to a reaction kettle, and the mixture was kept insulated from moisture and stirred continuously at room temperature. 33 parts by weight of trimethylsilanol were slowly added dropwise at a rate of 1 drop per second. After the addition was completed, the mixture was kept insulated from moisture and stirred for 120 minutes. Then, low molecular weight was removed at 75° C., and the mixture was cooled to obtain a reactant. The stirring speed was 500 rpm.

[0109] 3) 100 parts by weight of P48V20000 is added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 4 parts by weight of the reactants are added, and the mixture is stirred at 40° C. for 120 minutes under vacuum at a stirring speed of 500 rpm to obtain an ethoxy-terminated chain extender. In the ethoxy-terminated chain extender, R7 is an aniline methyl group, and R8 is —O—Si(CH3)3.

[0110] 4) 80 parts by weight of the end-capped polymer and 20 parts by weight of the ethoxy end-capped chain extender are added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 1 part by weight of methyltriethoxysilane, 2 parts by weight of 3-aminopropyltriethoxysilane and 8 parts by weight of fumed silica S150 (dried) are added, and the mixture is vacuumed and stirred for 30 minutes, and then 0.5 parts by weight of dibutyltin dilaurate is added, and the mixture is vacuumed and stirred for 30 minutes, wherein the stirring speed is 500 rpm, to obtain a single-component deethanol-type silicone sealant composition.

[0111] Example 2

[0112] The composition formula and preparation method are basically the same as those in Example 1, except that 8 parts by weight of fumed silica S150 in step 4) are replaced with 90 parts by weight of calcium carbonate CCS-25 (pre-dried to a moisture content of <0.1%).

[0113] Example 3

[0114] The composition formula and preparation method are basically the same as those of Example 1, except that 80 parts by weight of the end-capped polymer and 20 parts by weight of the ethoxy end-capped chain extender in step 4) are replaced with 50 parts by weight of the end-capped polymer and 50 parts by weight of the ethoxy end-capped chain extender.

[0115] Example 4

[0116] The composition formula and preparation method are basically the same as those in Example 1, except that the aniline methyl triethoxysilane in step 3) is replaced with an equimolar amount of diethylamino methyl triethoxysilane. In the prepared ethoxy-terminated chain extender, R7 is diethylamino methyl, and R8 is -O-Si(CH3)3.

[0117] Example 5

[0118] 1) 50 parts by weight of P48V5000 and 50 parts by weight of P48V1500 are added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 10 parts by weight of diethylaminomethyltriethoxysilane are added, and vacuum is drawn at room temperature and stirred for 120 minutes to obtain an ethoxy-terminated polymer, wherein the stirring speed is 500 rpm. In the ethoxy-terminated polymer, R1 and R2 are methyl groups, and R3 is a diethylaminomethyl group.

[0119] 2) 100 parts by weight of diethylaminomethyltriethoxysilane was added to the reaction kettle, and the mixture was kept insulated from moisture and stirred continuously at room temperature. 36 parts by weight of trimethylsilanol was slowly added dropwise at a rate of 1 drop per second. After the addition was completed, the mixture was kept insulated from moisture and stirred for 120 minutes. Then, the low molecular weight was removed at 65° C., and the mixture was cooled to obtain a reactant. The stirring speed was 500 rpm.

[0120] 3) 100 parts by weight of P48V750 is added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 10 parts by weight of the reactant is added, and the mixture is stirred for 120 minutes under vacuum at room temperature to obtain an ethoxy-terminated chain extender. In the ethoxy-terminated chain extender, R7 is diethylaminomethyl and R8 is -O-Si(CH3)3.

[0121] 4) 70 parts by weight of the end-capped polymer and 30 parts by weight of the ethoxy end-capped chain extender are added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 2 parts by weight of methyltriethoxysilane and 10 parts by weight of fumed silica 812S are added, and the mixture is vacuumed and stirred for 30 minutes, and then 0.5 parts by weight of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane and 0.1 parts by weight of dibutyltin dilaurate are added, and the mixture is vacuumed and stirred for 30 minutes at a stirring speed of 500 rpm to obtain a one-component deethanol-type silicone sealant composition.

[0122] Example 6

[0123] 1) 70 parts by weight of L621V20000 and 30 parts by weight of L621V1000 are added to a reactor equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 2 parts by weight of triethoxysilane and 20 ppm of chloroplatinic acid hexahydrate are added, and the mixture is reacted at 50° C. under nitrogen protection for 24 hours to obtain an ethoxy-terminated polymer, wherein the stirring speed is 500 rpm. In the ethoxy-terminated polymer, R4 and R5 are methyl groups, and R6 is an ethoxy group.

[0124] 2) 60 parts by weight of the end-capped polymer and 40 parts by weight of the ethoxy end-capped chain extender prepared in Example 5 were added to a high-speed stirring kettle equipped with a nitrogen system, a vacuum system and a heating and cooling system, and then 1 part by weight of methyltriethoxysilane and 10 parts by weight of fumed silica 812S were added, and the mixture was vacuumed and stirred for 30 minutes, and then 1 part by weight of N-(β-aminoethyl)-γ-aminopropyltriethoxysilane and 0.3 parts by weight of dibutyltin dilaurate were added, and the mixture was vacuumed and stirred for 30 minutes, wherein the stirring speed was 500 rpm, to obtain a single-component deethanol-type silicone sealant composition.

[0125] Example 7

[0126] The composition formula and preparation method are basically the same as those in Example 5, except that the diethylaminomethyltriethoxysilane in step 3) is replaced with an equimolar amount of dichloromethyltriethoxysilane, and 0.5% of butanone oxime by total weight is added to accelerate the reaction rate. In the obtained ethoxy-terminated chain extender, R7 is dichloromethyl and R8 is -O-Si(CH3)3.

[0127] Comparative Example 1

[0128] The composition formula and preparation method are basically the same as those in Example 1, except that step 3) is not performed, and the ethoxy end-capping chain extender in step 4) is replaced by an equal weight portion of methyl silicone oil H47V1000.

[0129] Comparative Example 2

[0130] The composition formula and preparation method are basically the same as those in Example 1, except that the P48V80000 in step 1) is replaced with an equal amount of H48V80000.

[0131] Comparative Example 3

[0132] The composition formula and preparation method are basically the same as those in Example 5, except that step 3) is not performed, and the ethoxy end-capping chain extender in step 4) is replaced with an equal weight portion of methyl silicone oil H47V1000.

[0133] Comparative Example 4

[0134] The composition formula and preparation method are basically the same as those of Example 6, except that the triethoxysilane in step 1) is replaced with an equimolar amount of trimethoxysilane.

[0135] Comparative Example 5

[0136] The composition formula and preparation method are basically the same as those in Example 5, except that the diethylaminomethyltriethoxysilane in step 2) is replaced with an equal molar amount of methyltriethoxysilane.

[0137] Comparative Example 6

[0138] The composition formula and preparation method are basically the same as those of Example 5, except that the diethylaminomethyltriethoxysilane in step 2) is replaced with an equimolar amount of vinyltriethoxysilane.

[0139] Comparative Example 7

[0140] The composition formula and preparation method are basically the same as those in Example 5, except that the ethoxy end-capping chain extender in step 4) is replaced by an equal weight amount of dimethyldiethoxysilane.

[0141] Comparative Example 8

[0142] The composition formula and preparation method are basically the same as those of Example 5, except that 30 parts by weight of the ethoxy-terminated chain extender in step 4) is replaced with 3 parts by weight of dimethyldiethoxysilane, and the amount of the terminated polymer is adjusted to 97 parts by weight accordingly.

[0143] Comparative Example 9

[0144] The composition formula and preparation method are basically the same as those of Example 5, except that 30 parts of the ethoxy-terminated chain extender in step 4) are replaced by an equal weight portion of the ethoxy-terminated polymer prepared in step 1).

[0145] Comparative Example 10

[0146] The composition formula and preparation method are basically the same as those in Example 5, except that the P48V5000, P48V1500 and P48V750 used are all replaced by H48V135000 in equal weight.

[0147] Comparative Example 11

[0148] The composition formula and preparation method are basically the same as those of Example 6, except that the amounts of the end-capping polymer and the ethoxy end-capping chain extender in step 2) are adjusted to 40 parts by weight and 60 parts by weight, respectively.

[0149] Performance Testing

[0150] The compositions of the embodiments and comparative examples were tested according to the following standards:

[0151] The surface drying time is tested according to GB / T 13477;

[0152] The tensile strength is tested according to GB / T 528 (Type 2 specimen);

[0153] The elongation at break is tested according to GB / T 528 (Type 2 specimen);

[0154] The modulus of 100% stretch is tested according to GB / T 528 (Type 2 specimen);

[0155] Hardness is tested according to GB / T 531.

[0156] The test results of the compositions of various embodiments and comparative examples are shown in Table 1.

[0157] Table 1 Performance test results

[0158]

[0159]

[0160] From the test data of the examples and comparative examples, it can be seen that: Examples 1-2 and 4-7 all have fast surface drying speed, low modulus, low hardness, high elongation, and the cured release substances are all ethanol, and the cyclosiloxane content meets the SVHC standard, which is environmentally friendly and healthy; Example 3 has good performance except for the slow surface drying speed, and can also meet some applications. Comparative Examples 1 and 3 replace the reactive chain extender with non-reactive silicone oil, and the modulus is significantly higher than that of the corresponding examples, and the elongation at break is also lower than that of the corresponding examples; Comparative Example 2 uses α,ω-dihydroxy polydimethylsiloxane with a high ring body content to prepare ethoxy-terminated polymers, and the overall ring body content exceeds the standard and does not meet the SVHC standard; Comparative Example 4 uses trimethoxysilane to prepare methoxy-terminated polymers, and the final product releases methanol during the curing process, which does not meet the health and environmental protection requirements; Although Comparative Examples 5 and 6 also prepare chain extenders in the same way, the R7 group in their chain extenders is different from that protected by the patent of the present invention, and the modulus and hardness are higher than those of Example 5, while the elongation at break is lower than that of Example 5. The reason is It may be that the R7 group has low activity. On the one hand, it is difficult to obtain a high-purity difunctional product during the preparation process. On the other hand, due to its low activity, the chain extension effect is poor; Comparative Example 7 uses dimethyldiethoxysilane, and the amount used is too much, which causes the glue to be sticky for a long time and not solidify; Comparative Example 8 reduces the amount of dimethyldiethoxy and can be cured normally, but also due to its low activity, the chain extension effect is not obvious; Comparative Example 9 does not use a chain extender, the strength, hardness, and modulus are improved, and the elongation at break is reduced; Comparative Example 10 uses a polymer with too high viscosity, which makes it impossible to produce and use the glue normally; Comparative Example 11 has a large proportion of chain extender, the glue surface dries slowly, the strength is low, the hardness is too low, the modulus is too low, and the elongation at break is not significantly improved.

Claims

1. A one-component alcohol-free silicone sealant composition, wherein: The sealant composition comprises 100 parts by weight of a base glue, 1 to 150 parts by weight of a reinforcing filler, 1 to 10 parts by weight of a cross-linking agent, and 0.01 to 5 parts by weight of a catalyst; wherein the base glue comprises an ethoxy-terminated polymer and an ethoxy-terminated chain extender, the ethoxy-terminated polymer comprises at least one selected from the polymers represented by formula I and formula II, the ethoxy-terminated chain extender comprises a polymer represented by formula III, and the weight ratio of the ethoxy-terminated polymer to the ethoxy-terminated chain extender is 8:2 to 5:5; Formula I In formula I, R1 and R2 are the same or different and are independently selected from methyl, ethyl and phenyl; R3 is selected from methyl, vinyl, diethylaminomethyl, anilinomethyl, aminopropyl, aminoethylaminopropyl and ethoxy; m is in the range of 100 to 5000; Formula II In formula II, R4 and R5 are the same or different and are independently selected from methyl, ethyl and phenyl; R6 is selected from methyl and ethoxy; X is -CH2CH2-; n is in the range of 100 to 5000; Formula III In formula III, R7 is selected from diethylaminomethyl, dichloromethyl and anilinemethyl; R8 is selected from methyl, propyl, vinyl and -O-Si(CH3)3; and a ranges from 10 to 3000.

2. The sealant composition according to claim 1, wherein: The content of cyclosiloxane in the sealant composition is less than 1000 ppm.

3. The sealant composition according to claim 1, wherein: The viscosity of the ethoxy-terminated polymer at 25° C. is 500 to 100,000 cps; and / or, The range of m is 200 to 2000; and / or the range of n is 200 to 2000.

4. The sealant composition according to claim 1, wherein: The viscosity of the ethoxylated end-capping chain extender at 25° C. is 10 to 50,000 cps; and / or, The range of a is 50 to 1500.

5. The sealant composition according to claim 1, wherein: The reinforcing filler is selected from precipitated silica, fumed silica, hydrophobic treated silica, nano-activated calcium carbonate, heavy calcium carbonate, carbon nanotubes, graphene, glass fiber, silicate, nano-montmorillonite and mixtures thereof; and / or, The crosslinking agent is selected from the group consisting of tetraethyl orthosilicate, polyethyl orthosilicate, methyltriethoxysilane, vinyltriethoxysilane, 3-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane and mixtures thereof; and / or, The catalyst is selected from the group consisting of organotin, organotin chelate, titanate, titanate chelate, organobismuth, aminosilane and mixtures thereof.

6. The sealant composition according to claim 5, wherein: The catalyst is selected from the group consisting of titanate catalysts, titanate chelates, dibutyltin dilaurate, dibutyltin diacetate and mixtures thereof.

7. The sealant composition according to claim 1, wherein: The sealant composition further comprises: 1-80 parts by weight of flame retardant filler; and / or 10 to 1000 parts by weight of thermally conductive filler; and / or 0.1 to 8 parts by weight of coupling agent; and / or 0.1 to 8 parts by weight of pigment; and / or Plasticizer 1~8 parts by weight.

8. The sealant composition according to claim 7, wherein: The flame retardant filler is selected from aluminum hydroxide, magnesium hydroxide, carbon flame retardant, nitrogen-phosphorus flame retardant, phosphorus-silicon flame retardant, platinum-containing flame retardant and mixtures thereof; and / or, The thermally conductive filler is selected from aluminum hydroxide, aluminum oxide, zinc oxide, cerium oxide, aluminum nitride, boron nitride, silicon nitride, silicon carbide, graphene, carbon nanotubes, quartz powder, aluminum powder, copper powder, silver powder and mixtures thereof; and / or, The coupling agent is selected from 3-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane, dodecyltriethoxysilane, hexadecyltriethoxysilane, anilinemethyltriethoxysilane and mixtures thereof; and / or, The plasticizer is selected from methyl silicone oil, phenyl silicone oil, vinyl silicone oil and a mixture thereof.

9. The method for preparing the sealant composition according to any one of claims 1 to 8, wherein: The preparation method comprises the following steps: uniformly mixing a base glue, a reinforcing filler, a cross-linking agent, a catalyst, an optional flame retardant filler, an optional thermal conductive filler, an optional coupling agent, an optional pigment and an optional plasticizer under moisture isolation, stirring for 15 to 180 minutes at a temperature of 10 to 60° C. and a negative pressure of -0.085 to -0.099 MPa, and optionally cooling to room temperature to obtain a single-component deethanol-type silicone sealant composition.

10. The method for preparing the sealant composition according to claim 9, wherein: Stir for 20 to 60 minutes at a temperature of 20 to 50°C and a negative pressure of -0.085 to -0.099 MPa.

11. The preparation method according to claim 9, wherein: The preparation method of the ethoxy-terminated polymer shown in Formula I comprises the following steps: S100, at 10-150° C., under the protection of an inert gas, in the presence of an optional condensation catalyst, allowing a silane crosslinking agent A containing at least two ethoxy groups to undergo a condensation reaction with a terminal hydroxyl polysiloxane; The condensation reaction time in step S100 is 2-36h; The structure of the silane crosslinking agent A containing at least two ethoxy groups in step S100 is shown in Formula IV, Formula IV In formula IV, R3 is selected from methyl, vinyl, diethylaminomethyl, phenylaminomethyl, aminopropyl, aminoethylaminopropyl and ethoxy; R 10 is ethyl; In step S100, the condensation catalyst is selected from butanone oxime; and / or, based on the weight of the hydroxy-terminated polysiloxane, the condensation catalyst is used in an amount of 0.001 to 1% by weight; In step S100, the weight ratio of the terminal hydroxyl polysiloxane to the silane crosslinking agent A containing at least two ethoxy groups is 100:(1-20); The inert gas in step S100 is nitrogen, helium or argon; And / or, the method for preparing the ethoxy-terminated polymer shown in formula II comprises the following steps: S200, at 10-150° C., under the protection of an inert gas, in the presence of an optional addition catalyst, allowing a silane crosslinking agent B containing at least two ethoxy groups to undergo an addition reaction with a vinyl-terminated polysiloxane; The addition reaction time in step S200 is 2-36h; The silane crosslinking agent B containing at least two ethoxy groups in step S200 is triethoxysilane or methyldiethoxysilane; The addition catalyst in step S200 is selected from chloroplatinic acid or Custer platinum catalyst; and / or, based on the weight of the vinyl-terminated polysiloxane, the amount of the addition catalyst is 0.0001-0.01% by weight; In step S200, the weight ratio of the vinyl-terminated polysiloxane to the silane crosslinking agent B containing at least two ethoxy groups is 100:(1-20); The inert gas in step S200 is nitrogen, helium or argon.

12. The preparation method according to any one of claims 9 to 11, wherein: In formula III, R8 is -O-Si(CH3)3, and the preparation method of the ethoxy-terminated chain extender comprises the following steps: S310, adding the same amount of trimethylsilanol to diethylaminomethyltriethoxysilane, anilinemethyltriethoxysilane or dichloromethyltriethoxysilane at 10-50°C in a moisture-proof condition, reacting for 90-180 minutes, raising the temperature to 50-80°C, removing the generated ethanol under negative pressure, and obtaining an intermediate product; S320, react the intermediate product with terminal hydroxyl polysiloxane at 10-50°C under the protection of inert gas for 90-180 minutes, then raise the temperature to 50-80°C, remove the generated ethanol under negative pressure, and obtain an ethoxy-terminated chain extender.

13. The preparation method according to claim 12, wherein: In step S320, the weight ratio of the intermediate product to the hydroxyl-terminated polysiloxane is 2 to 10:100; The reaction in step S320 is carried out in the presence of a catalyst; The inert gas in step S320 is nitrogen, helium or argon.

14. The preparation method according to claim 12, wherein: The catalyst used in step S320 is selected from organic tin, titanate, acid, base, amino compound, butanone oxime.