A kind of steel for heavy truck engine bearing and its production method

Through the optimization of vacuum degassing continuous casting process, the problem of insufficient wear resistance and mechanical properties of heavy truck engine bearing materials is solved, and high purity and high mechanical properties of steel are produced, which meets the efficient operation needs of heavy truck engines and reduces production cost.

CN117286399BActive Publication Date: 2024-11-19JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311037136.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-17
Publication Date
2024-11-19
Estimated Expiration
2043-08-17

AI Technical Summary

Technical Problem

The bearing materials of existing heavy truck engines have shortcomings in wear resistance, plasticity and mechanical properties, and it is difficult to meet the strict requirements for efficient operation of heavy truck engines.

Method used

Using vacuum degassing continuous casting technology with high cleanliness and high mechanical properties, the high purity and high mechanical properties of steel are used to optimize chemical composition and process design, and the harmful elements and inclusions in steel are reduced, thus improving the structural uniformity and mechanical properties of steel, and producing high purity and high quality. Carburized steel with mechanical properties.

Benefits of technology

It realizes high wear resistance, plasticity and high life of heavy truck engine bearing materials, reduces production costs, and meets the high performance requirements of heavy truck engine bearings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004399372380000041
    Figure BDA0004399372380000041
  • Figure BDA0004399372380000042
    Figure BDA0004399372380000042
  • Figure BDA0004399372380000061
    Figure BDA0004399372380000061
Patent Text Reader

Abstract

The invention relates to a steel for a heavy truck engine bearing and a production method thereof, belonging to the technical field of metallurgy. The chemical composition of the bearing steel is as follows: C: 0.17-0.21%, Si: 0.20-0.35%, Mn: 0.8-1.0%, Cr: 0.5-0.7%, Nb: 0.02-0.06%, V: 0.15-0.20%, S≤0.008%, P≤0.020%, Ni≤0.25%, Cu≤0.25%, Mo≤0.10%, Al≤0.05%, Ti≤0.003%, O≤0.0010%, As≤0.04%, Sn≤0.03%, Sb≤0.005%, Pb≤0.002%, and the remainder is Fe and unavoidable impurities. The bearing steel of this application is produced by vacuum degassing continuous casting, and electric furnace or converter, refining, and vacuum degassing are used to effectively remove harmful non-metallic inclusions to improve product purity. By optimizing the key parameters of continuous casting and rolling, an optimal production process is obtained, and finally steel with high purity, high mechanical properties and long life is obtained, and a new steel under the high-efficiency, large-capacity, low-cost, and high-quality production model is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to bearing steel and a production method thereof. Background Art

[0002] With the rapid development of my country's bearing industry, Chinese bearing enterprises have completed the transformation from high-speed bearing production growth to high-quality manufacturing, and from a large bearing production country to a strong bearing country by improving their independent innovation capabilities, technical research capabilities and innovative practice capabilities. my country's heavy-duty trucks have also developed rapidly with the strength of the bearing industry. Heavy-duty trucks have made technological innovations in many aspects such as efficient internal combustion engines, lightweight technology, and pure electric power systems. In the future, heavy-duty trucks should have the characteristics of high power, lightweight, and green energy saving. However, the heavy-duty truck engine is known as the "heart" of heavy-duty trucks, and its importance is self-evident. Among them, the heavy-duty truck engine bearing is its key component. In order to ensure the efficient and stable operation of the engine, the engine bearing material is required to have high hardness, high elastic limit, high contact fatigue strength and other characteristics. In order to achieve the above performance requirements, the requirements for the uniformity of chemical composition, the number and type of non-metallic inclusions, and the uniformity of organization of heavy-duty truck engine bearing materials are very strict. It is required that the heavy-duty truck engine bearing material has higher requirements than the conventional household car bearing material in terms of purity, mechanical properties, hardenability and other properties.

[0003] At present, the material usually used for heavy-duty truck engine bearings is GCr15, and the common processing methods are bar cutting-spheroidizing annealing-machining-quenching and tempering heat treatment-grinding. The biggest advantage of using GCr15 material is that the overall material hardenability and wear resistance are relatively good, but its overall mechanical properties are not good, and the core plasticity is relatively poor. Due to the special environment of heavy-duty truck engines, when the heavy-duty truck engine combustion chamber is working, there is a relatively large variable ratio inside the engine, so the heavy-duty truck engine bearings not only require the bearing material to have high wear resistance, but also require good plasticity.

[0004] Based on the above information required for heavy-duty truck engine bearing materials, the carburizing steel for heavy-duty truck engine bearings of the present invention has the characteristics of high wear resistance, plasticity and long life. The present invention adopts a high cleanliness and high mechanical property vacuum degassing continuous casting process route. At the same time, a unique design is made on the material composition, and finally a new steel that meets the requirements of heavy-duty truck engine bearings is produced. Summary of the invention

[0005] In order to meet the requirements of high wear resistance, plasticity and high mechanical properties of steel for heavy-duty truck engine bearings, the present invention adopts a vacuum degassing continuous casting process route with high cleanliness and high mechanical properties, and specially designs the chemical composition. It utilizes vacuum degassing, continuous casting and continuous rolling to produce in a high-efficiency, high-capacity and low-cost production mode, and adopts special control means to reduce harmful elements and inclusions in steel and improve the purity of molten steel. The internal organization of the steel is controlled by optimizing the design of each continuous casting and continuous rolling process, thereby improving the uniformity of the steel organization and producing steel for heavy-duty truck engine bearings with high purity and high mechanical properties.

[0006] The chemical composition of the steel for heavy truck engine bearing of the present invention is designed as follows: C: 0.17-0.21%, Si: 0.20-0.35%, Mn: 0.8-1.0%, Cr: 0.5-0.7%, Nb: 0.02-0.06%, V: 0.15-0.20%, S≤0.008%, P≤0.020%, Ni≤0.25%, Cu≤0.25%, Mo≤0.10%, Al≤0.05%, Ti≤0.003%, O≤0.0010%, As≤0.04%, Sn≤0.03%, Sb≤0.005%, Pb≤0.002%, and the balance is Fe and unavoidable impurities.

[0007] 1) Determination of C content

[0008] C is an element necessary to ensure the wear resistance of steel. Increasing the carbon content in steel will increase its martensitic transformation ability, thereby increasing its hardness and strength, and further improving wear resistance. However, too high a C content is not good for the toughness of steel. In addition, too high a C content will also lead to severe center segregation, thereby affecting the core toughness of the steel. The present invention controls its content to 0.17-0.21%.

[0009] 2) Determination of Si content

[0010] Adding Si to steel can strengthen ferrite, improve strength, elastic limit and hardenability, but too much Si will cause intergranular oxidation during carburizing heat treatment, affecting the carburizing quality. The Si content of the present invention is determined to be in the range of 0.20-0.35%.

[0011] 3) Determination of Mn content

[0012] Mn, as a deoxidizing element in the steelmaking process, can improve the hardenability of steel. Mn can also fix the form of sulfur in steel and form MnS and (Fe, Mn)S, which are less harmful to steel performance, and reduce or inhibit the formation of FeS. Therefore, manganese in steel can improve the purity and performance of steel. At the same time, manganese plays the role of solid solution strengthening and grain refinement in steel to improve strength and significantly improve hardenability; however, if the manganese content is too high, it will promote the growth of austenite grains in steel. The range of Mn content in the present invention is determined to be 0.8-1.0%.

[0013] 4) Determination of Cr content

[0014] Cr is a carbide-forming element that can improve the hardenability, wear resistance and corrosion resistance of steel. However, if the Cr content is too high, the hardness of the steel will be too high, which is not conducive to customer processing and use. Based on the above analysis, the Cr content of the present invention is determined to be within the range of 0.5-0.7%.

[0015] 5) Determination of Al content

[0016] Al is added as a deoxidizing element in steel. In addition to reducing the dissolved oxygen in molten steel, Al and N form dispersed and fine aluminum nitride to refine the grains. However, when the Al content is too high, large particles of Al2O3 and other brittle inclusions are easily formed during the molten steel smelting process, which reduces the purity of the molten steel and affects the service life of the steel. The range of the Al content in the present invention is determined to be ≤0.05%.

[0017] 6) Determination of Nb content

[0018] The solute dragging effect of Nb and the pinning effect of Nb (C, N) on the austenite grain boundary both inhibit the recrystallization of deformed austenite, expand the non-recrystallization range of austenite, and reduce the waiting time for round bar production. Nb has a strong binding force with carbon, nitrogen, and oxygen, and forms extremely stable compounds with them, so it can refine the grains, reduce the overheating sensitivity and temper brittleness of steel, and at the same time improve the thermal strength of steel. Therefore, Nb is determined to be 0.02~0.06%.

[0019] 7) Determination of V content

[0020] V is an element that effectively refines grains, which can improve the strength and toughness of steel. In addition, the carbides formed by vanadium and carbon can improve corrosion resistance at high temperatures. Therefore, V is determined to be 0.04-0.07%.

[0021] 8) Determination of Ti content

[0022] Ti harms bearings by remaining in the steel in the form of titanium nitride and titanium carbonitride inclusions. Such inclusions are hard and angular, seriously affecting the fatigue life of the bearings. Ti inclusions not only reduce the fatigue life of the bearings, but also affect the roughness of the bearings. The range of Ti content in the present invention is determined to be ≤0.003%.

[0023] 9) Determination of O content

[0024] Oxygen naturally enters the steel during the steelmaking process, and the oxygen remaining in the steel at a later stage mainly exists in the form of FeO, MnO, SiO2, Al2O3 and other inclusions. In particular, Al2O3 inclusions affect the service life of steel. A large number of tests have shown that reducing the oxygen content is significantly beneficial to improving the purity of steel, especially reducing the content of oxide brittle inclusions (mainly Al2O3 inclusions) in steel grades. The range of the O content in the present invention is determined to be ≤0.0010%.

[0025] 10) Determination of P and S content

[0026] Phosphorus causes serious segregation during solidification in steel. Phosphorus dissolves in ferrite to cause grain distortion and coarsening, and increases cold brittleness. The range of Phosphorus content in the present invention is determined to be ≤0.020%. Sulfur causes hot brittleness in steel, reduces the ductility and toughness of steel, but Sulfur can improve the cutting performance of steel. The range of Sulfur content in the present invention is determined to be ≤0.008%.

[0027] 11) Determination of As, Sn, Sb and Pb contents

[0028] Trace elements such as As, Sn, Sb, and Pb are all low-melting-point nonferrous metals. Their presence in steel causes soft spots on the surface of parts and uneven hardness. Therefore, they are regarded as harmful elements in steel. The content range of these elements in the present invention is determined as As≤0.04%, Sn≤0.03%, Sb≤0.005%, and Pb≤0.002%.

[0029] The present invention has strict requirements on microscopic inclusions, macroscopic inclusions and mechanical properties. Microscopic inclusions are mainly brittle inclusions of type B and type D. Brittle inclusions are hard particles in steel, which produce various stress concentrations when the bearing is running. At the same time, they are easy to separate from the matrix and produce cracks during the deformation process of the steel, which further aggravates the stress concentration and easily causes cracking. The larger the inclusion particles and the longer the length, the greater the harm.

[0030] The non-metallic inclusions of the present invention are tested according to the GB / T 10561A method, and the levels of various inclusions do not exceed the requirements of Table 1.

[0031] Table 1

[0032]

[0033] The macro defects of the present invention are inspected by the water immersion high frequency flaw detection method according to SEP 1927 (water immersion ultrasonic determination method for purity of forged steel bars), and the length of a single inclusion does not exceed 3mm, and the defect index does not exceed 10mm / dm 3 .

[0034] The uniformity and density of the macrostructure of steel affect the life of the bearing. The present invention requires the use of ASTM E381 to grade the macrostructure of steel, requiring S≤2, R≤2, C≤2, and no shrinkage cavities, cracks or subcutaneous bubbles are allowed.

[0035] In order to ensure the strength and toughness of the steel, the present invention puts forward requirements on the grain size, and the rating is carried out according to DIN EN ISO643, requiring the grain size to be ≥ grade 6; in order to ensure that it is suitable for use in heavy-duty truck engine bearings, the steel of the present invention puts forward requirements on mechanical properties, and the mechanical properties are tested according to GB / T228. The specific requirements are shown in Table 2 below.

[0036] Table 2

[0037]

[0038] The present invention discloses a production method for heavy truck engine bearing steel, and the process flow is converter or electric furnace → ladle refining furnace LF furnace → vacuum circulating degassing furnace RH or VD furnace → continuous casting CCM (large cross section) → hot rolling → finishing → surface and internal flaw detection → packaging.

[0039] The main steps are as follows:

[0040] (1) Molten steel smelting:

[0041] Converter or electric furnace: Add high-quality molten iron (the preferred composition of molten iron is P≤0.100%, S≤0.050%) and scrap steel into the converter or electric furnace for primary smelting, blow oxygen to the top of the furnace mouth to assist melting, and blow argon to the bottom for stirring. Preferably: the oxygen blowing amount per ton of steel is 20 cubic meters to 30 cubic meters, and the argon gas amount per ton of steel is 1 cubic meter to 1.5 cubic meters. Add an active composite slag-making agent (CaO-MgO) to react with harmful elements in steel to remove harmful elements phosphorus (P≤0.020%) and titanium (Ti≤0.003%). The final carbon when tapping from the primary smelting furnace is 0.12% to 0.15%, and the tapping temperature is ≥1630°C. Slag blocking is used for tapping, and some alloys are added during tapping (initial adjustment of composition). Slag removal is performed immediately after tapping. After slag removal, it is quickly hoisted to the refining LF furnace for smelting.

[0042] Refining furnace: The whole refining process adopts argon protective atmosphere smelting. During the process, Al particles and CaO-SiC-CaF2 high-performance composite slag-making agent are used for deoxidation and removal of harmful non-metallic inclusions. Aluminum particles enter the deep part of molten steel for precipitation deoxidation, and CaO-SiC-CaF2 high-performance composite slag-making agent diffuses deoxidation on the surface of molten steel and adsorbs and removes harmful non-metallic inclusions. During the smelting process, Al particles (30-50 kg) are first fed into the molten steel, and then CaO-SiC-CaF2 high-performance composite slag-making agent (300-500 kg) is added at one time. Argon is connected to the bottom of the ladle, and then the electrode is inserted into the slag for submerged arc power supply. The power is turned off every 15 minutes, and the temperature of the molten steel is measured and sampled for analysis. The required main elements are added according to the target requirements. The number of temperature measurement and sampling of the refining furnace is controlled at 3-4 times until the composition meets the product requirements. The temperature of the refining furnace is controlled at 1550-1580℃, the refining time is controlled at more than 40min, and the soft blowing time of molten steel is ≤10min.

[0043] Vacuum degassing: During RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, and the vacuum circulation treatment time of molten steel is maintained at ≥20min to ensure that harmful gases in the steel are effectively removed. After the vacuum treatment, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of the molten steel is ≤10min. At the same time, a 50m silicon-calcium wire is fed to denature the Al2O3 inclusions in the molten steel, and Al2O3 or MgO·A12O3 is denatured into calcium aluminate and composite inclusions with lower melting points to ensure smooth subsequent pouring.

[0044] (2) Continuous casting: Argon protection is used throughout the casting process to prevent secondary contamination and oxidation of the molten steel; preferably, low superheat casting is used (superheat △T≤15°C); the amount of molten steel in the tundish is controlled at 20-25 tons, and the light pressure control technology (pressure reduction 8mm-10mm) is used, and the casting speed is 0.7-0.9m / min; an appropriate steel flow to water ratio (1.2-1.3L / kg) is used; during the continuous casting process, a composite electromagnetic stirring of crystallizer electromagnetic stirring MEMS + solidification end electromagnetic stirring FEMS is used. Through the above various control technologies, the center segregation of steel is further improved and the uniformity of steel structure is improved.

[0045] (3) Heating rolling: The continuous casting billet is conveyed to a heating furnace in a neutral or weakly oxidizing atmosphere by a roller, heated and rolled into round bars. The specific rolling process is as follows: the continuous casting billet enters a step-beam heating furnace through a conveying roller, the air-to-coal ratio of the furnace gas is controlled at 0.98-1.02 to reduce the residual oxygen content, the steel is heated to 1050-1150°C in the heating furnace, the holding time is 3h-4h, the continuous casting billet start rolling temperature is controlled at 950-1000°C, and a five-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass), and the five-pass reduction amounts are 20%-25%, 15%-20%, 20%-25%, 20%-25%, 15%-20%, respectively, so that the core structure of the casting billet is deformed and recrystallized first during the deformation process, so that the central structure of the steel is more uniform and dense under the action of large pressure. Then it is rolled alternately through 16 horizontal and vertical rolling mills, and finally the round bars with specifications of φ20mm~φ60mm are rolled.

[0046] (4) Finishing: including straightening, chamfering and other finishing processes to ensure that indicators such as size and curvature meet the requirements.

[0047] (5) The surface and interior are subjected to 100% non-destructive testing, and only those that pass the inspection can be considered qualified products.

[0048] Compared with the prior art, the advantages of the present invention are:

[0049] 1) The present invention adopts the design of high mechanical property carburizing steel in the composition design, and adds trace alloy elements Nb and V to improve the wear resistance, strength and toughness of the steel. Compared with the existing product GCr15, the production cost of the steel of the present invention is greatly reduced. In terms of performance, it has the high strength and high wear resistance of GCr15, and also has high mechanical properties, meeting the requirements of heavy truck engine bearing steel.

[0050] 2) The present invention uses special steelmaking and rolling processes to ensure the purity and mechanical properties of steel, thereby better meeting the requirements for material use. DETAILED DESCRIPTION

[0051] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0052] The chemical composition (wt%) of the steel for heavy truck engine bearings in various embodiments of the present invention is shown in Table 3 and Table 4.

[0053] Table 3

[0054] C Si Mn P S Cr Cu Ni Al Embodiment 1 of the present invention 0.19 0.30 0.91 0.008 0.005 0.59 0.01 0.02 0.022 Embodiment 2 of the present invention 0.19 0.29 0.92 0.007 0.004 0.6 0.02 0.03 0.019 Embodiment 3 of the present invention 0.20 0.31 0.90 0.008 0.005 0.59 0.01 0.02 0.020

[0055] Table 4

[0056] Mo Nb V As Sn Sb Pb Ti O Embodiment 1 of the present invention 0.01 0.030 0.16 0.0052 0.0019 0.0014 0.001 0.0009 0.00059 Embodiment 2 of the present invention 0.01 0.028 0.17 0.0054 0.0015 0.0012 0.001 0.0010 0.00060 Embodiment 3 of the present invention 0.01 0.033 0.17 0.0053 0.0016 0.0013 0.001 0.0010 0.00058

[0057] Table 5 Inclusions in the steel materials of each example

[0058]

[0059] Table 6 Macro data of steel materials in various examples

[0060]

[0061]

[0062] Table 7 Grain size data of each example steel

[0063]

[0064] Table 8 Water immersion high frequency flaw detection data of steel materials in various embodiments

[0065]

[0066] Table 9 Mechanical properties data of steel materials in various embodiments

[0067]

[0068] A production method for heavy-duty truck engine bearing steel according to an embodiment of the present invention has a process flow of converter or electric furnace → ladle refining furnace LF furnace → vacuum circulating degassing furnace RH or VD furnace → continuous casting CCM (large cross-section) → hot rolling → finishing → surface and internal flaw detection → packaging.

[0069] Specifically, in the production process of electric furnace / converter, the oxygen blowing amount per ton of steel is 23 / 25 / 26 cubic meters, the argon gas amount per ton of steel is 1.25 / 1.30 / 1.33 cubic meters, the tapping end point C is controlled at 0.12%-0.15%, the end point P is controlled at ≤0.020%, the end point Ti≤0.003%, the tapping temperature is controlled at 1632℃-1638℃, the slag blocking system is used for tapping, and some alloys are added during tapping (initial adjustment of composition). After the molten steel is completely discharged, the slag is removed and then quickly hoisted to the refining LF furnace; to the LF For the refining furnace, first, place the ladle cover over the molten steel, pass argon gas through the ladle cover to protect the molten steel, add Al particles (30-50 kg) into the molten steel, and then add CaO-SiC-CaF2 high-performance composite slag-making agent (300-500 kg) at one time. Connect argon gas to the bottom of the ladle, and then insert the electrode into the slag for submerged arc power supply. Cut off the power every 15 minutes, measure the temperature of the molten steel and take samples for analysis, add the required main elements according to the target requirements, and control the number of temperature measurement and sampling of the refining furnace to 3-4 times until the composition meets the product requirements. The temperature of the refining furnace is controlled at 1550-1580℃, the refining time is 45-50min, and the soft blowing time of molten steel is 5-10min; during RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, the vacuum circulation treatment time of molten steel is ≥20min, the soft blowing time of molten steel is ≤10min, and 50m of silicon-calcium wire is fed at the same time; the continuous casting superheat is controlled within ≤15℃, the continuous casting pulling speed is controlled at 0.7-0.9m / min, the light pressure reduction is 8mm-10mm, the molten steel volume in the tundish is controlled at 20-25 tons, the steel flow water volume is controlled at 1.2-1.3L / kg, and the composite electromagnetic stirring of crystallizer electromagnetic stirring MEMS + solidification end electromagnetic stirring FEMS is adopted; the continuous casting billet is passed through The conveyor roller enters a walking-beam heating furnace in a neutral or weakly oxidizing atmosphere, and the air-coal ratio of the furnace gas is controlled at 0.98-1.02. The steel is heated to 1050-1150°C in the heating furnace, and the insulation time is 3h-4h. The rolling temperature of the continuous casting billet after being discharged from the furnace is 950-1000°C. The continuous casting billet adopts a five-pass reciprocating turning large reduction technology (the steel is turned 90° after each pass), and the five-pass reduction amounts are 20%-25%, 15%-20%, 20%-25%, 20%-25%, and 15%-20% respectively, and then it is rolled alternately through 16 horizontal and vertical rolling mills, and finally the round bars with a specification of Φ20mm-Φ60mm are rolled, and slowly cooled to room temperature after going off the line, and then the bars are subjected to subsequent flaw detection and finishing.

[0070] It can be seen from Tables 3, 4, 5, 6, 7, 8 and 9 that the heavy-duty truck engine bearing steel in each embodiment of the present invention has the control level of harmful elements such as phosphorus, oxygen, titanium and non-metallic inclusions reaching the international advanced level. From the results of macroscopic inspection, mechanical properties and microstructure grain size, the macroscopic quality, mechanical properties, microstructure uniformity and density of the present invention all meet the requirements of heavy-duty truck engine bearing steel.

[0071] At the same time, each embodiment was subjected to water immersion high frequency flaw detection according to the SEP 1927 method, and the macro inclusions reached zero defects.

[0072] In summary, the present invention adopts the vacuum degassing continuous casting process to produce the heavy-duty truck engine bearing steel and its production method. In terms of purity, the electric furnace or converter, refining, and vacuum degassing processes are adopted to effectively remove harmful non-metallic inclusions. In terms of organizational uniformity and mechanical properties, a set of optimal production processes are obtained by optimizing the key parameters of continuous casting and rolling, and finally a steel with high purity, high mechanical properties and long life is obtained, producing a new steel with high efficiency, large capacity, low cost and high quality production model.

[0073] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A method for producing steel for heavy truck engine bearings, characterized in that: The chemical composition of the steel is as follows by mass percentage: C: 0.19-0.20%, Si: 0.29-0.31%, Mn: 0.90-0.92%, Cr: 0.59-0.60%, Nb: 0.028-0.033%, V: 0.16-0.17%, S≤0.008%, P≤0.020%, Ni: 0.02-0.03%, Cu: 0.01-0.02%, Mo: 0.01%, Al: 0.019-0. 022%, Ti: 0.0009~0.0010%, O≤0.0010%, As≤0.04%, Sn≤0.03%, Sb≤0.005%, Pb≤0.002%, the balance is Fe and unavoidable impurities; mechanical properties are tested according to GB / T228: the diameter of the sample blank is 25mm, heat treatment: normalizing temperature is 910±10℃, meeting the following requirements: tensile strength Rm≥500MPa, elongation A≥30%, and section shrinkage Z≥55%; The steel production method comprises:

1. Molten steel smelting: (1.1) Primary refining in converter or electric furnace: molten iron and scrap steel are added to converter or electric furnace for primary refining. Oxygen is blown at the top of the furnace mouth to assist melting, argon is blown at the bottom for stirring, and an active composite slag-making agent is added to react with harmful elements in the steel to dephosphorize and detitanium the molten steel: P≤0.020%, Ti≤0.003%, the final carbon of the molten steel at the time of tapping: 0.12%~0.15%, the tapping temperature ≥1630℃, slag is blocked during tapping, and some alloys are added during tapping. Slag removal is carried out immediately after tapping is completed. After slag removal, the slag is quickly hoisted to the refining furnace for refining; (1.2) Refining in refining furnace: The whole refining process adopts argon protective atmosphere smelting. During the process, Al particles and CaO-SiC-CaF2 high-performance composite slag-making agent are used for deoxidation and removal of harmful non-metallic inclusions. Aluminum particles enter the deep part of molten steel for precipitation deoxidation, and CaO-SiC-CaF2 high-performance composite slag-making agent diffuses deoxidation on the surface of molten steel and adsorbs and removes harmful non-metallic inclusions. During the refining process, 30-50 kg of Al particles are first fed into the molten steel, and then 300-50 kg of Al particles are added at one time. 00Kg of CaO-SiC-CaF2 high-performance composite slag-making agent, argon gas is connected to the bottom of the ladle, and then the electrode is inserted into the slag for submerged arc power supply. The power is cut off every 10-20 minutes, the temperature of the molten steel is measured and sampled for analysis, and the required alloy elements are added according to the target requirements. The number of temperature measurement and sampling of the refining furnace is controlled at 3-4 times until the composition meets the design requirements, the temperature of the refining furnace is controlled at 1550-1580℃, the refining time is controlled at more than 40 minutes, and the soft blowing time of the molten steel is ≤10 minutes; (1.3) Vacuum degassing: During RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, and the vacuum cycle treatment time of the molten steel is maintained for ≥20min. After the vacuum treatment is completed, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of the molten steel is ≤10min. At the same time, a silicon-calcium wire is fed to denature the Al2O3 inclusions in the molten steel; 2. Continuous casting: The whole process adopts argon protection pouring to prevent secondary contamination and oxidation of molten steel, and low superheat pouring is adopted: superheat △T≤15℃; the amount of molten steel in the tundish is controlled at 20-25 tons, and the light pressure control technology is adopted: the pressure is 8mm-10mm, the pouring speed is 0.7-0.9m / min; the steel flow water volume is 1.2-1.3L / kg; the composite electromagnetic stirring of crystallizer electromagnetic stirring MEMS + solidification end electromagnetic stirring FEMS is adopted in the continuous casting process; 3. Heating and rolling: The continuous casting billet is conveyed to a heating furnace with a neutral or weakly oxidizing atmosphere through a roller table for heating and rolling into round bars: The continuous casting billet is heated in a heating furnace, and the air-coal ratio of the furnace gas is controlled at 0.98-1.02, heated to 1050°C-1150°C, and kept warm for 3h-4h. The rolling start temperature of the continuous casting billet is controlled at 950-1000°C. A five-pass reciprocating turning large reduction rolling process is adopted. After each pass, the steel is turned 90°. The five-pass reduction amounts are 20%-25%, 15%-20%, 20%-25%, 20%-25%, 15%-20% respectively, and then rolled alternately through 16 horizontal and vertical rolling mills to roll the billet into round bars with specifications of Φ20mm-Φ60mm.

2. The method according to claim 1, characterized in that: Non-metallic inclusions in the organization are tested according to GB / T 10561A method, and the levels of various inclusions are: A fine series ≤1.5, A coarse series ≤1.0, B fine series ≤1.0, B coarse series ≤0.5, C fine series ≤0, C coarse series ≤0, D fine series ≤1.0, D coarse series ≤0.5, DS ≤1.0; Macro defects in the organization are inspected according to the SEP 1927 water immersion high frequency flaw detection method. The length of a single inclusion does not exceed 3mm, and the defect index does not exceed 10mm / dm 3 ; ASTM E381 is used to grade the macrostructure of steel, which meets S≤2, R≤2, C≤2, and no shrinkage cavities, cracks or subcutaneous bubbles appear; Grain size rating is carried out according to DIN EN ISO643, with grain size ≥ grade 6.

3. The method according to claim 1, characterized in that: In step 1.1, P≤0.100% and S≤0.050% in the molten iron; during smelting, the oxygen blowing amount per ton of steel is 20-30 cubic meters, and the argon gas amount per ton of steel is 1-1.5 cubic meters; and CaO-MgO active composite slag-making agent is added to remove P and S in the steel.

4. The method according to claim 1, characterized in that: After rolling, the round steel bars are finished, including straightening and chamfering.