A high-toughness aluminum alloy coated steel plate and preparation method thereof

By adding alloy elements to the aluminum alloy-coated steel plate and optimizing the hot-dip plating process, the problem of insufficient deformation ability and corrosion resistance of the coating is solved, and an aluminum alloy-coated steel plate with high toughness and excellent corrosion resistance is achieved, which is suitable for complex deformation and Stamping and forming.

CN117305711BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311305952.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-10
Publication Date
2024-10-22
Estimated Expiration
2043-10-10

AI Technical Summary

Technical Problem

The deformation ability and corrosion resistance of existing aluminum-silicon coated steel plates during the stamping process need to be improved, and the coating strength and toughness are insufficient.

Method used

By adding alloying elements such as Si, Mg, Cu, Mn, Fe, Zn, Ti, etc. to the coating and optimizing the hot dip plating process, the content of alloying elements and the refinement of the coating structure can be controlled to improve the toughness and corrosion resistance of the coating. The cooling process is adjusted to reduce the strength and hardness of the coating and enhance formability.

Benefits of technology

It achieves high toughness, good formability and excellent corrosion resistance of the coating. The hardness of the coating ranges from HV50 to HV160. It has good formability, weldability and machinability, and the corrosion resistance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004486194860000051
    Figure BDA0004486194860000051
  • Figure BDA0004486194860000052
    Figure BDA0004486194860000052
Patent Text Reader

Abstract

The present invention relates to a high-toughness aluminum alloy coated steel plate and a preparation method thereof. The alloy elements in the coating are calculated by mass percentage as follows: Si 0.5% to 9.0%, Mg 0.8% to 3.0%, Cu 0.1% to 5.0%, Mn 0.1% to 0.4%, Fe 0.5% to 2.4%, Zn 1% to 10%, Ti 0.11% to 2.50%, and the rest are Al and inevitable impurities. A high-toughness aluminum alloy coated steel plate and a preparation method thereof. The aluminum alloy coated steel plate produced by the method has good forming performance, good coating toughness, and the coated steel plate has excellent corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum alloy coated steel plate production, and in particular relates to a high-toughness aluminum alloy coated steel plate and a preparation method thereof. Background Art

[0002] The existing aluminum-silicon coated steel plate is made by adding about 10% Si element to aluminum plating. Although hot-dip plating of aluminum alloy coating is achieved, the strength and toughness of the coating needs to be further improved, especially the deformation ability of the coating during stamping forming needs to be further improved.

[0003] The present invention adopts a method combining adding alloy elements and optimizing hot-dip plating process to improve the toughness and corrosion resistance of the aluminum alloy coating, refine the coating structure, and further improve the forming performance of the coating. Summary of the invention

[0004] The present invention provides a high-toughness aluminum alloy coated steel plate and a preparation method thereof. The aluminum alloy coated steel plate produced by the method has good forming performance, good coating toughness, and the coated steel plate has excellent corrosion resistance.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A high-toughness aluminum alloy coated steel plate, wherein the alloy elements in the coating are calculated by mass percentage as follows: Si 0.5%-9.0%, Mg 0.8%-3.0%, Cu 0.1%-5.0%, Mn 0.1%-0.4%, Fe 0.5%-2.4%, Zn 1%-10%, Ti 0.11%-2.50%, and the rest are Al and unavoidable impurities.

[0007] The chemical elements in the steel plate include, by mass percentage: C 0.001% to 0.38%, Si 0.01% to 0.80%, Mn 0.10% to 2.50%, P≤0.08%, S≤0.05%, Al 0.02% to 1.00%, Ti≤0.08%, B≤0.005%, Cr≤0.70%, and the rest are Fe and unavoidable impurities.

[0008] The chemical elements in the steel plate also include one or more of the following elements: Mo 0.10% to 0.80%, Cu≤1.00%, Ni 0.4% to 1.0%, and Nb≤0.05%.

[0009] The coating hardness is HV50~HV160. The coating contains MgZn2 and Mg2Si precipitates, which is suitable for complex deformation such as stamping. The coating has excellent deformation ability, and there is no visible crack in the cold-bent 0T coating.

[0010] A method for preparing a high-toughness aluminum alloy coated steel plate, comprising smelting, casting, hot rolling, pickling, cold rolling, and hot-dip plating;

[0011] The hot rolling process is: heating at 1240±50℃, keeping warm for 190±50 minutes, rough rolling at 1100±50℃, finishing rolling at 1050±50℃, final rolling at 880±50℃, and coiling at 450~800℃;

[0012] Hot dip plating process: hot dip plating of cold rolled substrate, heating annealing temperature is controlled at 700-900℃, temperature of entering aluminum pot is 630-700℃, temperature of aluminum pot is 630-690℃;

[0013] The post-plating cooling process is as follows: immediately after exiting the aluminum pot and the air knife, the coating temperature is cooled to 600±5℃ at a cooling rate of 10±5℃ / s, and then immediately cooled to 400±10℃ at a rate of 20±5℃ / s, and then cooled to 270±20℃ at a rate of 10±5℃ / s, entering the turning roller, air-cooling to below 100℃, entering water cooling, and after reaching room temperature, the coated steel plate is heated in the post-processing area at a temperature of 200±60℃ for more than 5 seconds.

[0014] The present invention adds 0.5%-9.0% Si, 0.8%-3.0% Mg, 0.1%-5.0% Cu, 0.1%-0.4% Mn, 0.5%-2.4% Fe, 1%-10% Zn and 0.11%-2.50% Ti alloy elements into the coating, which can refine the coating structure and improve the toughness of the coating. At the same time, due to the upper limit control of the content of the alloy elements, it can ensure that the coating has higher plastic toughness, reduce the strength and hardness of the coating, and improve the forming performance.

[0015] In addition, adding 0.8% to 3.0% Mg and 1% to 10% Zn to the coating can greatly improve the corrosion resistance of the coating.

[0016] The temperature of the zinc pot of the present invention is 630-690° C., and good surface quality can be obtained after the zinc pot is taken out, thereby avoiding defects such as zinc flow ripples.

[0017] Immediately after the zinc pot and air knife are removed, the coating temperature is cooled to 600±5℃ at a cooling rate of 10±5℃ / s. The purpose is to cool at a slower temperature in the temperature range from the zinc pot temperature to 600±5℃, reduce the air volume of the air knife, and improve the surface quality; then immediately cool to 400±10℃ at a rate of 20±5℃ / s, quickly cool in this temperature range, refine the coating structure, and improve the toughness of the coating; then cool to 270±20℃ at a rate of 10±5℃ / s, enter the turning roller, air cool to below 100℃, enter water cooling, enter the turning roller at 270±20℃, the coating has a certain hardness, and the roller mark and scratch are avoided. After reaching room temperature, the coated steel plate is heated in the post-treatment area at a temperature of 200±60℃ for more than 5 seconds. The purpose is to make the precipitated phases such as Mg2Si and MgZn2 separate from the coherent and semi-coherent relationship with the aluminum alloy matrix, reduce the strength and hardness of the coating, and improve the forming performance.

[0018] The role of elements in the coating:

[0019] Al is the main element of aluminum alloy coating, which can provide good protection for steel plates during storage, use and parts after forming, form aluminum-rich phases in the coating structure, and form intermetallic compounds with other alloy elements in the coating.

[0020] Si is enriched in the intermetallic compound layer to form a compact inhibition layer structure, reduce the thickness of the alloy layer, improve the toughness of the coating, refine the structure of the coating, improve the coating performance, and form intermetallic compounds such as Mg2Si with Mg element.

[0021] Mg improves the corrosion resistance of the coating, forms intermetallic compounds such as Mg2Si with Si, and forms intermetallic compounds such as MgZn2 with Zn, refines the coating structure, and improves the toughness of the coating.

[0022] The addition of Ti can provide more nucleation sites and refine the microstructure of the coating. The addition of Si and Ti at the same time can generate a more compact inhibition layer and improve the uniformity of coating growth.

[0023] Mn can provide more nucleation points, reduce the size of aluminum flowers, improve the corrosion resistance of the coating, refine the grains, and improve the toughness of the coating. It can also reduce the adverse effects of Fe in the plating solution.

[0024] Cu improves the toughness of the coating, refines the coating structure, and forms intermetallic compounds with coating elements: Al2Cu, Al2CuMg, etc.

[0025] Fe is an element that must be avoided in the coating, and it can improve the bonding strength between the coating and the substrate.

[0026] Zn improves the corrosion resistance of the coating, forms intermetallic compounds such as MgZn2 with Mg, refines the coating structure, and improves the toughness of the coating.

[0027] The role of elements in steel:

[0028] As the main alloying element, C contributes most to the strength of steel; Mn and Si can provide solid solution strengthening effect and improve the quenching performance of steel.

[0029] To ensure hardenability, Ti, Cr and B are also added.

[0030] The addition of Cu improves the corrosion resistance of steel, thereby preventing the penetration of H and improving the delayed fracture resistance of steel. The addition of Mo and Nb strengthens the steel matrix and refines the grains.

[0031] The addition of Si and Al can inhibit the formation of cementite.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention provides an aluminum alloy coated steel plate, the coating hardness of which is HV50-HV160, the coating contains MgZn2 and Mg2Si precipitates, has good formability, weldability, and machinability, and also has medium strength and excellent corrosion resistance. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with embodiments. The following embodiments are used to specifically illustrate the contents of the present invention. These embodiments are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.

[0035] The embodiments are shown in Tables 1 to 4, wherein Table 1 is the chemical element composition of the coating of the embodiment; Table 2 is the chemical composition of the steel of the embodiment; Table 3 is the hot rolling and hot dip plating process parameters of the steel of the embodiment; Table 4 is the post-plating cooling process and performance of the steel of the embodiment.

[0036] Table 1 Chemical element composition of coatings of Examples 1-14

[0037] Si Ti Cu Fe Mn Mg Zn Al 1 1.0 0.5 0.5 1.5 0.15 0.9 1.5 margin 2 2.0 0.11 1 1.6 0.11 1.0 1.8 margin 3 3.0 0.12 0.6 2.2 0.18 1.5 1.5 margin 4 4.0 0.13 0.5 1.8 0.21 1.8 2 margin 5 5.0 0.14 0.7 2 0.22 2.5 3 margin 6 6.0 0.15 0.8 1.2 0.23 2.6 3.5 margin 7 7.0 0.16 0.9 1.1 0.4 2.3 9 margin 8 8.0 1.0 1.1 1 0.25 3.2 4 margin 9 8.8 0.17 2 1.9 0.34 3.4 4.5 margin 10 7.5 2.0 1.2 2.0 0.33 2.0 5 margin 11 6.5 1.1 2.4 2.1 0.3 3.6 6 margin 12 5.5 1.2 2.8 2.3 0.2 3 7 margin 13 4.5 1.5 3 1.7 0.32 2.2 8 margin 14 3.5 2.4 4 1.4 0.31 2.7 9.8 margin

[0038] Table 2 Chemical composition of steels of Examples 1-14

[0039] C Si Mn Al Ni Cu Cr Mo B Nb Ti P S Fe 1 0.001 0.01 0.10 0.01 0 0 0 0 0 0.03 0.06 0.015 0.010 margin 2 0.002 0.02 0.12 0.02 0 0 0 0 0 0.02 0.05 0.012 0.008 margin 3 0.02 0.02 0.15 0.03 0 0 0.15 0 0.002 0 0 0.020 0.009 margin 4 0.03 0.01 0.18 0.04 0 0 0 0 0.003 0 0 0.011 0.005 margin 5 0.06 0.03 0.20 0.05 0 0.2 0 0 0 0 0.06 0.012 0.008 margin 6 0.07 0.02 1.21 0.06 0 0 0.05 0 0.005 0 0.04 0.006 0.003 margin 7 0.14 0.10 0.35 0.88 0 0 0.03 0 0.003 0.03 0 0.007 0.004 margin 8 0.15 0.15 0.50 0.95 0 0.5 0.40 0.20 0.002 0.05 0 0.008 0.005 margin 9 0.18 0.18 0.80 0.5 0.5 0.8 0.50 0 0.004 0 0.02 0.009 0.006 margin 10 0.20 0.25 1.00 0.6 0 0 0 0 0.005 0.08 0.04 0.010 0.007 margin 11 0.22 0.28 1.25 0.05 0.2 0.2 0.80 0.40 0.003 0.02 0.03 0.015 0.008 margin 12 0.28 0.30 1.50 0.04 0.2 0 0 0 0.002 0.03 0.04 0.018 0.009 margin 13 0.30 0.35 1.60 0.03 0 0 0 0 0.004 0 0.05 0.020 0.013 margin 14 0.35 0.40 2.00 0.02 1.0 0 0 0 0.003 0.05 0 0.025 0.015 margin

[0040] Table 3 Hot rolling and hot dip coating process parameters of steels in Examples 1-14

[0041]

[0042] Table 4 Post-plating cooling process and performance parameters of steels of Examples 1-14

[0043]

[0044] The coating of the steel plate has good toughness, excellent formability and good corrosion resistance. The corrosion resistance of all coatings meets the following requirements: the double-sided 80g coating thickness salt spray test will not produce red rust for more than 4500 hours.

Claims

1. A high-toughness aluminum alloy coated steel plate, characterized in that: The alloy elements in the coating are calculated by mass percentage as follows: Si 0.5% to 9.0%, Mg 0.8% to 3.0%, Cu 0.1% to 5.0%, Mn 0.1% to 0.4%, Fe 0.5% to 2.4%, Zn 1.5% to 10%, Ti 0.11% to 2.50%, and the rest are Al and unavoidable impurities; The coating hardness is HV50~HV160, and the coating contains MgZn2 and Mg2Si precipitates; The cooling process of the steel plate after plating is as follows: after exiting the aluminum pot and the air knife, the coating temperature is cooled to 600±5℃ at a cooling rate of 10±5℃ / s, and then cooled to 400±10℃ at a rate of 20±5℃ / s, and then cooled to 270±20℃ at a rate of 10±5℃ / s, entering the turning roller, air-cooling to below 100℃, entering water cooling, and after reaching room temperature, the coated steel plate is heated in the post-processing area at a temperature of 200±60℃ for more than 5 seconds.

2. The high-toughness aluminum alloy coated steel plate according to claim 1, characterized in that: The chemical elements in the steel plate include, by mass percentage: C 0.001%~0.38%, Si 0.01%~0.80%, Mn 0.10%~2.50%, P≤0.08%, S≤0.05%, Al 0.02%~1.00%, Ti≤0.08%, B≤0.005%, Cr≤0.70%, and the rest are Fe and unavoidable impurities.

3. The high-toughness aluminum alloy coated steel plate according to claim 2, characterized in that: The chemical elements in the steel plate also include one or more of the following elements: Mo 0.10%~0.80%, Cu≤1.00%, Ni 0.4%~1.0%, Nb≤0.05%.

4. A method for preparing a high-toughness aluminum alloy coated steel plate as claimed in any one of claims 1 to 3, comprising smelting, casting, hot rolling, pickling, cold rolling and hot-dip plating; characterized in that: Hot dip plating process: hot dip plating of cold rolled substrate, heating annealing temperature is controlled at 700-900℃, temperature of entering aluminum pot is 630-700℃, temperature of aluminum pot is 630-690℃; The post-plating cooling process is as follows: after exiting the aluminum pot and the air knife, the coating temperature is cooled to 600±5℃ at a cooling rate of 10±5℃ / s, and then cooled to 400±10℃ at a rate of 20±5℃ / s, and then cooled to 270±20℃ at a rate of 10±5℃ / s, entering the turning roller, air-cooling to below 100℃, entering water cooling, and after reaching room temperature, the coated steel plate is heated in the post-processing area at a temperature of 200±60℃ for more than 5 seconds.

5. The method for preparing a high-toughness aluminum alloy coated steel plate according to claim 4, characterized in that: The hot rolling process is: heating at 1240±50℃, keeping warm for 190±50 minutes, rough rolling at 1100±50℃, finishing rolling at 1050±50℃, final rolling at 880±50℃, and coiling at 450~800℃.